General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 - 7.98 g/cm³ Show Material materials with Densidad of 7.9 - 7.98 g/cm³ |
50.0 °C | 7.96 g/cm³ Show Material materials with Densidad of 7.96 g/cm³ | |
100.0 °C | 7.94 g/cm³ Show Material materials with Densidad of 7.94 g/cm³ | |
150.0 °C | 7.92 g/cm³ Show Material materials with Densidad of 7.92 g/cm³ | |
200.0 °C | 7.9 g/cm³ Show Material materials with Densidad of 7.9 g/cm³ | |
250.0 °C | 7.88 g/cm³ Show Material materials with Densidad of 7.88 g/cm³ | |
300.0 °C | 7.86 g/cm³ Show Material materials with Densidad of 7.86 g/cm³ | |
350.0 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | |
400.0 °C | 7.81 g/cm³ Show Material materials with Densidad of 7.81 g/cm³ | |
450.0 °C | 7.79 g/cm³ Show Material materials with Densidad of 7.79 g/cm³ | |
500.0 °C | 7.76 g/cm³ Show Material materials with Densidad of 7.76 g/cm³ | |
550.0 °C | 7.74 g/cm³ Show Material materials with Densidad of 7.74 g/cm³ | |
600.0 °C | 7.71 g/cm³ Show Material materials with Densidad of 7.71 g/cm³ | |
650.0 °C | 7.68 g/cm³ Show Material materials with Densidad of 7.68 g/cm³ | |
700.0 °C | 7.66 g/cm³ Show Material materials with Densidad of 7.66 g/cm³ | |
750.0 °C | 7.63 g/cm³ Show Material materials with Densidad of 7.63 g/cm³ | |
800.0 °C | 7.61 g/cm³ Show Material materials with Densidad of 7.61 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
50.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
100.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
150.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
350.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
450.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
550.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
600.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
650.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
700.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
750.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
800.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
Elongación A80 transversal | 20.0 °C | 35 % Show Material materials with Elongación A80 transversal of 35 % |
Elongación transversal | 20.0 °C | 35 % Show Material materials with Elongación transversal of 35 % |
Límite elástico Rp 0,2 | 50.0 °C | 191 MPa Show Material materials with Límite elástico Rp 0,2 of 191 MPa |
100.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | |
150.0 °C | 166 MPa Show Material materials with Límite elástico Rp 0,2 of 166 MPa | |
200.0 °C | 157 MPa Show Material materials with Límite elástico Rp 0,2 of 157 MPa | |
250.0 °C | 147 MPa Show Material materials with Límite elástico Rp 0,2 of 147 MPa | |
300.0 °C | 137 MPa Show Material materials with Límite elástico Rp 0,2 of 137 MPa | |
350.0 °C | 132 MPa Show Material materials with Límite elástico Rp 0,2 of 132 MPa | |
400.0 °C | 128 MPa Show Material materials with Límite elástico Rp 0,2 of 128 MPa | |
450.0 °C | 123 MPa Show Material materials with Límite elástico Rp 0,2 of 123 MPa | |
500.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | |
550.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | |
600.0 °C | 113 MPa Show Material materials with Límite elástico Rp 0,2 of 113 MPa | |
Límite elástico Rp 1,0 | 50.0 °C | 227 MPa Show Material materials with Límite elástico Rp 1,0 of 227 MPa |
100.0 °C | 205 MPa Show Material materials with Límite elástico Rp 1,0 of 205 MPa | |
150.0 °C | 195 MPa Show Material materials with Límite elástico Rp 1,0 of 195 MPa | |
200.0 °C | 186 MPa Show Material materials with Límite elástico Rp 1,0 of 186 MPa | |
250.0 °C | 176 MPa Show Material materials with Límite elástico Rp 1,0 of 176 MPa | |
300.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | |
350.0 °C | 162 MPa Show Material materials with Límite elástico Rp 1,0 of 162 MPa | |
400.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | |
450.0 °C | 152 MPa Show Material materials with Límite elástico Rp 1,0 of 152 MPa | |
500.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | |
550.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | |
600.0 °C | 142 MPa Show Material materials with Límite elástico Rp 1,0 of 142 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 200 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 200 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 240 MPa |
Módulo de cizallamiento | 20.0 °C | 77.01 - 78.09 GPa Show Material materials with Módulo de cizallamiento of 77.01 - 78.09 GPa |
50.0 °C | 77.3 GPa Show Material materials with Módulo de cizallamiento of 77.3 GPa | |
100.0 °C | 75.73 GPa Show Material materials with Módulo de cizallamiento of 75.73 GPa | |
150.0 °C | 73.87 GPa Show Material materials with Módulo de cizallamiento of 73.87 GPa | |
200.0 °C | 71.91 GPa Show Material materials with Módulo de cizallamiento of 71.91 GPa | |
250.0 °C | 69.95 GPa Show Material materials with Módulo de cizallamiento of 69.95 GPa | |
300.0 °C | 67.89 GPa Show Material materials with Módulo de cizallamiento of 67.89 GPa | |
350.0 °C | 65.83 GPa Show Material materials with Módulo de cizallamiento of 65.83 GPa | |
400.0 °C | 63.96 GPa Show Material materials with Módulo de cizallamiento of 63.96 GPa | |
450.0 °C | 62.1 GPa Show Material materials with Módulo de cizallamiento of 62.1 GPa | |
500.0 °C | 60.33 GPa Show Material materials with Módulo de cizallamiento of 60.33 GPa | |
550.0 °C | 58.57 GPa Show Material materials with Módulo de cizallamiento of 58.57 GPa | |
600.0 °C | 56.9 GPa Show Material materials with Módulo de cizallamiento of 56.9 GPa | |
650.0 °C | 55.33 GPa Show Material materials with Módulo de cizallamiento of 55.33 GPa | |
700.0 °C | 53.86 GPa Show Material materials with Módulo de cizallamiento of 53.86 GPa | |
750.0 °C | 52.29 GPa Show Material materials with Módulo de cizallamiento of 52.29 GPa | |
800.0 °C | 50.82 GPa Show Material materials with Módulo de cizallamiento of 50.82 GPa | |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | |
50.0 °C | 197.57 GPa Show Material materials with Módulo elástico of 197.57 GPa | |
100.0 °C | 190 - 193.65 GPa Show Material materials with Módulo elástico of 190 - 193.65 GPa | |
150.0 °C | 189.43 GPa Show Material materials with Módulo elástico of 189.43 GPa | |
200.0 °C | 182 - 185 GPa Show Material materials with Módulo elástico of 182 - 185 GPa | |
250.0 °C | 180.11 GPa Show Material materials with Módulo elástico of 180.11 GPa | |
300.0 °C | 174 - 175.5 GPa Show Material materials with Módulo elástico of 174 - 175.5 GPa | |
350.0 °C | 170.89 GPa Show Material materials with Módulo elástico of 170.89 GPa | |
400.0 °C | 166 - 170 GPa Show Material materials with Módulo elástico of 166 - 170 GPa | |
450.0 °C | 162.26 GPa Show Material materials with Módulo elástico of 162.26 GPa | |
500.0 °C | 158 - 160 GPa Show Material materials with Módulo elástico of 158 - 160 GPa | |
550.0 °C | 154.02 GPa Show Material materials with Módulo elástico of 154.02 GPa | |
600.0 °C | 149.99 - 155 GPa Show Material materials with Módulo elástico of 149.99 - 155 GPa | |
650.0 °C | 146.07 GPa Show Material materials with Módulo elástico of 146.07 GPa | |
700.0 °C | 142 - 145 GPa Show Material materials with Módulo elástico of 142 - 145 GPa | |
750.0 °C | 138.32 GPa Show Material materials with Módulo elástico of 138.32 GPa | |
800.0 °C | 134 - 140 GPa Show Material materials with Módulo elástico of 134 - 140 GPa | |
900.0 °C | 127 - 135 GPa Show Material materials with Módulo elástico of 127 - 135 GPa | |
1000.0 °C | 120 - 125 GPa Show Material materials with Módulo elástico of 120 - 125 GPa | |
Resistencia a la tracción | 20.0 °C | 510 - 690 MPa Show Material materials with Resistencia a la tracción of 510 - 690 MPa |
50.0 °C | 493 MPa Show Material materials with Resistencia a la tracción of 493 MPa | |
100.0 °C | 465 MPa Show Material materials with Resistencia a la tracción of 465 MPa | |
150.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | |
200.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | |
250.0 °C | 400 MPa Show Material materials with Resistencia a la tracción of 400 MPa | |
300.0 °C | 385 MPa Show Material materials with Resistencia a la tracción of 385 MPa | |
350.0 °C | 375 MPa Show Material materials with Resistencia a la tracción of 375 MPa | |
400.0 °C | 370 MPa Show Material materials with Resistencia a la tracción of 370 MPa | |
450.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | |
500.0 °C | 350 MPa Show Material materials with Resistencia a la tracción of 350 MPa | |
550.0 °C | 340 MPa Show Material materials with Resistencia a la tracción of 340 MPa | |
600.0 °C | 320 MPa Show Material materials with Resistencia a la tracción of 320 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 510 - 690 MPa Show Material materials with Resistencia a la tracción transversal of 510 - 690 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 450 - 472 J/(kg·K) Show Material materials with Calor específico of 450 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.63E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.63E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.69E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.69E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.73E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.73E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.78E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.78E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.82E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.82E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.85E-5 - 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 - 1.88E-5 1/K | ||
700.0 °C | 1.87E-5 - 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.87E-5 - 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.3 - 17 W/(m·K) Show Material materials with Conductividad térmica of 13.3 - 17 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Conductividad térmica of 14.9 W/(m·K) | ||
200.0 °C | 16.5 W/(m·K) Show Material materials with Conductividad térmica of 16.5 W/(m·K) | ||
300.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
400.0 °C | 19.5 W/(m·K) Show Material materials with Conductividad térmica of 19.5 W/(m·K) | ||
500.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
600.0 °C | 22.4 W/(m·K) Show Material materials with Conductividad térmica of 22.4 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
800.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.5 mm²/s Show Material materials with Difusividad térmica of 3.5 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Difusividad térmica of 5.1 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 800 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 800 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.1E-7 - 7.91E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.1E-7 - 7.91E-7 Ω·m |
50.0 °C | 7.61E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.61E-7 Ω·m | |
100.0 °C | 7.99E-7 - 8.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.99E-7 - 8.45E-7 Ω·m | |
150.0 °C | 8.38E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.38E-7 Ω·m | |
200.0 °C | 8.72E-7 - 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.72E-7 - 9.19E-7 Ω·m | |
250.0 °C | 9.04E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.04E-7 Ω·m | |
300.0 °C | 9.34E-7 - 9.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.34E-7 - 9.77E-7 Ω·m | |
350.0 °C | 9.63E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.63E-7 Ω·m | |
400.0 °C | 9.91E-7 - 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 9.91E-7 - 1.03E-6 Ω·m | |
450.0 °C | 1.02E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m | |
500.0 °C | 1.04E-6 - 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 - 1.08E-6 Ω·m | |
550.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
600.0 °C | 1.08E-6 - 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 - 1.12E-6 Ω·m | |
650.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
700.0 °C | 1.12E-6 - 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 - 1.15E-6 Ω·m | |
750.0 °C | 1.14E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
800.0 °C | 1.15E-6 - 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 - 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.04 - 0.1 % Show Material materials with Carbono of 0.04 - 0.1 % |
Cromo | 15 - 17 % Show Material materials with Cromo of 15 - 17 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Niobio | 1.2 % Show Material materials with Niobio of 1.2 % |
Níquel | 12 - 14 % Show Material materials with Níquel of 12 - 14 % |
Silicona | 0.3 - 0.6 % Show Material materials with Silicona of 0.3 - 0.6 % |
Titanio | 1.2 % Show Material materials with Titanio of 1.2 % |