General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Elongación | 12.1 % Show Material materials with Elongación of 12.1 % | Predicted Value, A80 | ||||
12.7 % Show Material materials with Elongación of 12.7 % | Predicted Value, A200 | |||||
17.9 % Show Material materials with Elongación of 17.9 % | Predicted Value, A5 | |||||
18.2 % Show Material materials with Elongación of 18.2 % | Predicted Value, A50 | |||||
18.3 % Show Material materials with Elongación of 18.3 % | Predicted Value, A80 Transverse | |||||
20 °C | 14 % Show Material materials with Elongación of 14 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 16 % Show Material materials with Elongación of 16 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
Estricción | 40.2 % Show Material materials with Estricción of 40.2 % | Predicted Value | ||||
44.8 % Show Material materials with Estricción of 44.8 % | Predicted Value, Transverse | |||||
Límite elástico | 308.9 MPa Show Material materials with Límite elástico of 308.9 MPa | Predicted Value, RP1 | ||||
329.7 MPa Show Material materials with Límite elástico of 329.7 MPa | Predicted Value, RP1 Transverse | |||||
502.3 MPa Show Material materials with Límite elástico of 502.3 MPa | Predicted Value, RP02 Transverse | |||||
541.7 MPa Show Material materials with Límite elástico of 541.7 MPa | Predicted Value, RP05 | |||||
723 MPa Show Material materials with Límite elástico of 723 MPa | Predicted Value, RP002 | |||||
20 °C | 630 MPa Show Material materials with Límite elástico of 630 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 650 MPa Show Material materials with Límite elástico of 650 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 690 MPa Show Material materials with Límite elástico of 690 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 690 MPa Show Material materials with Límite elástico of 690 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
100 °C | 660 MPa Show Material materials with Límite elástico of 660 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
150 °C | 640 MPa Show Material materials with Límite elástico of 640 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
200 °C | 605 MPa Show Material materials with Límite elástico of 605 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
250 °C | 585 MPa Show Material materials with Límite elástico of 585 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
300 °C | 570 MPa Show Material materials with Límite elástico of 570 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
350 °C | 550 MPa Show Material materials with Límite elástico of 550 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
400 °C | 530 MPa Show Material materials with Límite elástico of 530 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | RP02 | |
Módulo de cizallamiento | 79.6 GPa Show Material materials with Módulo de cizallamiento of 79.6 GPa | Predicted Value | ||||
Módulo elástico | 20 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
100 °C | 205 GPa Show Material materials with Módulo elástico of 205 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
200 °C | 198 GPa Show Material materials with Módulo elástico of 198 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
300 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
400 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
500 °C | 173 GPa Show Material materials with Módulo elástico of 173 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
Resistencia a la tracción | 20 °C | 710 - 940 MPa Show Material materials with Resistencia a la tracción of 710 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
20 °C | 710 - 930 MPa Show Material materials with Resistencia a la tracción of 710 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 710 - 900 MPa Show Material materials with Resistencia a la tracción of 710 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 760 - 940 MPa Show Material materials with Resistencia a la tracción of 760 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 760 - 930 MPa Show Material materials with Resistencia a la tracción of 760 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 760 - 900 MPa Show Material materials with Resistencia a la tracción of 760 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 770 - 940 MPa Show Material materials with Resistencia a la tracción of 770 - 940 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 770 - 930 MPa Show Material materials with Resistencia a la tracción of 770 - 930 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 770 - 900 MPa Show Material materials with Resistencia a la tracción of 770 - 900 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | ||
20 °C | 770 - 940 MPa Show Material materials with Resistencia a la tracción of 770 - 940 MPa | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat | Transverse | |
Resistencia al cizallamiento | 600.6 MPa Show Material materials with Resistencia al cizallamiento of 600.6 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
100 °C | 470 J/(kg·K) Show Material materials with Calor específico of 470 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
200 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
300 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
400 °C | 540 J/(kg·K) Show Material materials with Calor específico of 540 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
500 °C | 570 J/(kg·K) Show Material materials with Calor específico of 570 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
Coeficiente de dilatación térmica | 100 °C | 1.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
300 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
400 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
Conductividad térmica | 20 °C | 38 W/(m·K) Show Material materials with Conductividad térmica of 38 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
100 °C | 39 W/(m·K) Show Material materials with Conductividad térmica of 39 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
200 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
300 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
400 °C | 39 W/(m·K) Show Material materials with Conductividad térmica of 39 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
500 °C | 37 W/(m·K) Show Material materials with Conductividad térmica of 37 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 5 S/m Show Material materials with Conductividad eléctrica of 5 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | |
100 °C | 3.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
200 °C | 3.9e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.9e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
300 °C | 4.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
400 °C | 5.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.7e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat | ||
500 °C | 6.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.7e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10137-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.015 % Show Material materials with Aluminio of 0.015 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Boro | 0.005 % Show Material materials with Boro of 0.005 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Circonio | 0.12 % Show Material materials with Circonio of 0.12 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
0.15 % Show Material materials with Circonio of 0.15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Cromo | 1.5 % Show Material materials with Cromo of 1.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Manganeso | 1.6 % Show Material materials with Manganeso of 1.6 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
1.7 % Show Material materials with Manganeso of 1.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
Molibdeno | 0.6 % Show Material materials with Molibdeno of 0.6 % | quenched and tempered (+QT) | EN 10137-2 | Sheet, Flat |
0.7 % Show Material materials with Molibdeno of 0.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat | |
Niobio | 0.06 % Show Material materials with Niobio of 0.06 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Nitrógeno | 0.015 % Show Material materials with Nitrógeno of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Níquel | 2 % Show Material materials with Níquel of 2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Silicona | 0.8 % Show Material materials with Silicona of 0.8 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Vanadio | 0.12 % Show Material materials with Vanadio of 0.12 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, VdTÜV WB 257 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |