CEN/TS 13388 Grade CW106C R200, H065

Want to keep this datasheet? Save it now in your required format

Related Standards

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.9 g/cm³

Show Material materials with Density of 8.9 g/cm³

Dimension

PropertyValue

Dimensions

Durchmesser

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

112 GPa

Show Material materials with Elastic modulus of 112 GPa

Elongation

20.0 °C

30 %

Show Material materials with Elongation of 30 %

Hardness, Brinell

20.0 °C

65 - 90 [-]

Show Material materials with Hardness, Brinell of 65 - 90 [-]

Hardness, Vickers

20.0 °C

70 - 95 [-]

Show Material materials with Hardness, Vickers of 70 - 95 [-]

Tensile strength

20.0 °C

200 MPa

Show Material materials with Tensile strength of 200 MPa

Yield strength Rp0.2

20.0 °C

60 MPa

Show Material materials with Yield strength Rp0.2 of 60 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

20.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

100.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

Melting point

1070 - 1080 °C

Show Material materials with Melting point of 1070 - 1080 °C

Thermal conductivity

20.0 °C

167 - 320 W/(m·K)

Show Material materials with Thermal conductivity of 167 - 320 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

4.30E+7 S/m

Show Material materials with Electrical conductivity of 4.30E+7 S/m

Electrical resistivity

20.0 °C

2.33E-8 Ω·m

Show Material materials with Electrical resistivity of 2.33E-8 Ω·m

Chemical properties

PropertyValue

Chromium

0.5 - 1.2 %

Show Material materials with Chromium of 0.5 - 1.2 %

Iron

0.08 %

Show Material materials with Iron of 0.08 %

Other

Rest Cu, total 0.2

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

Zirconium

0.03 - 0.3 %

Show Material materials with Zirconium of 0.03 - 0.3 %

Technological properties

Property
Brazing

hard brazing : medium, soft brazing: medium

Workability

general (condition): good (solution annealed), medium (precipitation hardened)