Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.4 g/cm³

Show Material materials with Density of 8.4 g/cm³

Dimension

PropertyValue

Dimensions

Dicke

Mechanical

PropertyTemperatureValue

Elongation

20.0 °C

43 %

Show Material materials with Elongation of 43 %

Elongation A50

20.0 °C

33 %

Show Material materials with Elongation A50 of 33 %

Hardness, Vickers

20.0 °C

75 - 110 [-]

Show Material materials with Hardness, Vickers of 75 - 110 [-]

Tensile strength

20.0 °C

340 - 420 MPa

Show Material materials with Tensile strength of 340 - 420 MPa

Yield strength Rp0.2

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

Thermal

PropertyValue

Melting point

885 - 900 °C

Show Material materials with Melting point of 885 - 900 °C

Chemical properties

PropertyValue

Aluminium

0.05 %

Show Material materials with Aluminium of 0.05 %

Copper

60 - 61 %

Show Material materials with Copper of 60 - 61 %

Iron

0.2 %

Show Material materials with Iron of 0.2 %

Lead

1.6 - 2.5 %

Show Material materials with Lead of 1.6 - 2.5 %

Nickel

0.3 %

Show Material materials with Nickel of 0.3 %

Other

Rest Zn, total 0.2

Tin

0.2 %

Show Material materials with Tin of 0.2 %

Technological properties

Property
Brazing

hard brazing : good to medium, soft brazing: very good

Workability

Cold forming degree between anneals: max. 30 %, general (condition): medium