5052 O Non-Heat Treatable Al Wrought Alloy

Want to keep this datasheet? Save it now in your required format

Description

Universal work hardening alloy with medium strength, very good formability, very good corrosion resistance, and good durability properties.

Related Standards

Equivalent Materials

This material data has been provided by Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.68 g/cm³

Show Supplier Material materials with Density of 2.68 g/cm³

Dimension

PropertyValue

Thickness

0.2 - 6 mm

Show Supplier Material materials with Thickness of 0.2 - 6 mm

Mechanical

PropertyTemperatureValue

Bending angle 180°

23.0 °C

0 °/t

Show Supplier Material materials with Bending angle 180° of 0 °/t

Bending angle 90°

23.0 °C

0 °/t

Show Supplier Material materials with Bending angle 90° of 0 °/t

Elastic modulus

23.0 °C

70 GPa

Show Supplier Material materials with Elastic modulus of 70 GPa

Elongation A50

23.0 °C

12 %

Show Supplier Material materials with Elongation A50 of 12 %

Hardness, HBW

23.0 °C

47 [-]

Show Supplier Material materials with Hardness, HBW of 47 [-]

Shear modulus

23.0 °C

26.5 GPa

Show Supplier Material materials with Shear modulus of 26.5 GPa

Tensile strength

23.0 °C

170 - 215 MPa

Show Supplier Material materials with Tensile strength of 170 - 215 MPa

Yield strength

23.0 °C

65 MPa

Show Supplier Material materials with Yield strength of 65 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

2.4E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 2.4E-5 1/K

20-100°C

Thermal conductivity

23.0 °C

138 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 138 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

4.9E-8 Ω·m

Show Supplier Material materials with Electrical resistivity of 4.9E-8 Ω·m

Chemical properties

PropertyValue

Chromium

0.15 - 0.35 %

Show Supplier Material materials with Chromium of 0.15 - 0.35 %

Copper

0.1 %

Show Supplier Material materials with Copper of 0.1 %

Iron

0.4 %

Show Supplier Material materials with Iron of 0.4 %

Magnesium

2.2 - 2.8 %

Show Supplier Material materials with Magnesium of 2.2 - 2.8 %

Manganese

0.1 %

Show Supplier Material materials with Manganese of 0.1 %

Other

0.15 %

Show Supplier Material materials with Other of 0.15 %

Silicon

0.25 %

Show Supplier Material materials with Silicon of 0.25 %

Zinc

0.1 %

Show Supplier Material materials with Zinc of 0.1 %

Technological properties

Property
Anodizing

Excellent (anodizing quality)

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation

Corrosion properties

Excellent

Welding

Very Good

Workability

Good (in O temper)