8006 O Non-Heat Treatable Al Wrought Alloy

Want to keep this datasheet? Save it now in your required format

Description

High strength when compared to 1xxx in foil app. Alloy 8006 can be welded, adhesive bonded, and formed easily. It offers a useful combination of strength and ductility at room temperature while retaining its strength at elevated temperatures.

Related Standards

Equivalent Materials

This material data has been provided by Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.74 g/cm³

Show Supplier Material materials with Density of 2.74 g/cm³

Dimension

PropertyValue

Thickness

0.06 - 0.2 mm

Show Supplier Material materials with Thickness of 0.06 - 0.2 mm

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

70 GPa

Show Supplier Material materials with Elastic modulus of 70 GPa

Elongation A50

23.0 °C

14 %

Show Supplier Material materials with Elongation A50 of 14 %

Shear modulus

23.0 °C

25 GPa

Show Supplier Material materials with Shear modulus of 25 GPa

Tensile strength

23.0 °C

90 - 140 MPa

Show Supplier Material materials with Tensile strength of 90 - 140 MPa

Yield strength

23.0 °C

100 MPa

Show Supplier Material materials with Yield strength of 100 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

2.4E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 2.4E-5 1/K

20-100°C

Thermal conductivity

23.0 °C

190 - 210 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 190 - 210 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

3.1E-8 Ω·m

Show Supplier Material materials with Electrical resistivity of 3.1E-8 Ω·m

Chemical properties

PropertyValue

Copper

0.3 %

Show Supplier Material materials with Copper of 0.3 %

Iron

1.2 - 2 %

Show Supplier Material materials with Iron of 1.2 - 2 %

Magnesium

0.1 %

Show Supplier Material materials with Magnesium of 0.1 %

Manganese

0.3 - 1 %

Show Supplier Material materials with Manganese of 0.3 - 1 %

Silicon

0.4 %

Show Supplier Material materials with Silicon of 0.4 %

Zinc

0.1 %

Show Supplier Material materials with Zinc of 0.1 %

Technological properties

Property
Anodizing

Limited

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General applications; Tubes: Industrial tubes, Flexible tubes, Pipes; Insulation; Semi-rigid and corrugated: Pet food, Smooth wall; Components: Automotive fins, Heat exchangers

Corrosion properties

Limited

Welding

Good

Workability

Very Good