Standard properties of manufactured graphite include thermal stability, thermal conductivity, natural lubricity and chemical resistance to fluids. Flexible graphite combines these properties with the added characteristics of flexibility, compatibility, conformability and resilience. These characteristics differentiate flexible graphite from other forms of graphite, making it a superior, high-performance sealing material.

Properties

General

Bulk density ρbulk

1.12 g/cm³ at 20 °C

ASTM F-1315

Oxidation rate rox

0.75 g/m²·h at 500 °C

Show chart

Mechanical

Compressive modulus Ecomp

190 MPa at 20 °C

Compressive strength Rmc

165 MPa at 20 °C

ASTM C-695

Tensile strength Rm

5.2 MPa at 20 °C

ASTM F-152

Tow tensile strength Rm,two

190 MPa at 20 °C

Thermal

Max service temperature Tmax

3000 °C

Min service temperature Tmin

-240 °C

Electrical

Electrical resistivity ρel

8E-8 Ω·m at 20 °C

ASTM C-611

Chemical properties

Element

Weight %

Comment

C

99.9 %

ASTM C-695

S

0.05 %

Leco Method

Cl

5E-3 %

ASTM F-1277 (maximum leachable chlorides)

Technological properties

Application areas

Flexible Graphite has unique physical and chemical properties that make it ideal for sealing and for high-temperature applications, such as thermal radiation shielding. Flexible graphite is a distinctive material with the essential characteristics of graphite plus some unique properties which make it a valuable material for packings and gaskets.

This material data has been provided by Goodfellow.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.