HARDIALL® - TS 120 U - CuNi15Sn8 - C72900

Want to keep this datasheet? Save it now in your required format

Description

Hardiall® is a wrought spinodally hardened copper alloy CuNi15Sn8 (C72900) designed for high strength applications where toughness is required. It is non-magnetic and resists mechanical wear, galling, stress relaxation, corrosion and erosion. It is easily machined into complex components whilst being environmentally friendly being both lead and beryllium free.


Hardiall® is used within the aerospace, oil & gas and other industries thanks to its outstanding physical and mechanical properties in many varied components. Lebronze alloys has developed a full range of Hardiall® products to match it’s customers’ stringent needs. Lebronze Alloys manufacturing process for Hardiall® is fully integrated: internal processes include casting, hot and cold working stage, heat treatment and non-destructive testing. Being fully integrated ensures reactivity and complete traceability.

Equivalent Materials

This material data has been provided by Lebronze Alloys.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.95 g/cm³

Show Supplier Material materials with Density of 8.95 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

128 - 144 GPa

Show Supplier Material materials with Elastic modulus of 128 - 144 GPa

Elongation

23.0 °C

15 %

Show Supplier Material materials with Elongation of 15 %

Hardness, Brinell

23.0 °C

233 - 245 [-]

Show Supplier Material materials with Hardness, Brinell of 233 - 245 [-]

Hardness, Rockwell C

23.0 °C

22 - 24 [-]

Show Supplier Material materials with Hardness, Rockwell C of 22 - 24 [-]

Hardness, Vickers

23.0 °C

241 - 252 [-]

Show Supplier Material materials with Hardness, Vickers of 241 - 252 [-]

Tensile strength

23.0 °C

825 MPa

Show Supplier Material materials with Tensile strength of 825 MPa

Yield strength

23.0 °C

755 MPa

Show Supplier Material materials with Yield strength of 755 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.64E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.64E-5 1/K

for 20-200°C

Thermal conductivity

23.0 °C

38 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 38 W/(m·K)

for 20-200°C

Electrical

PropertyTemperatureValue

Electrical conductivity

23.0 °C

5.00E+6 S/m

Show Supplier Material materials with Electrical conductivity of 5.00E+6 S/m

Magnetic

PropertyTemperatureValueComment

Relative magnetic permeability

23.0 °C

1 [-]

Show Supplier Material materials with Relative magnetic permeability of 1 [-]

max

Technological properties

Property
Application areas

Hardiall® can be an alternative to Beryllium Copper for some applications. It is environment friendly, being Beryllium-free, Lead-free, and recyclable. Aerospace: friction bushings and bearings. In landing gears, bushings and bearings are required to operate under severe conditions, they need to be lubricated and replaced frequently causing recurring maintenance downtimes. To reduce maintenance costs, Hardiall® is used for such applications as it demonstrates excellent lubricity, wear, and galling resistance. Oil & Gas: couplings for onshore production systems e.g. sucker rods. Hardiall is also used in onshore oil pumps as sucker rod and valve rod guide bushing couplings. In such applications where stainless steel is generally used, Hardiall® demonstrates excellent resistance to metal-to-metal wear. Mining: bushings and bearings. In Mining equipment, bushings and bearings are highly solicited components. They need to be lubricated and replaced frequently implying recurrent production downtimes and maintenance man hours. Hardiall® is used in excavators, mining trucks and longwall shearers.

Corrosion properties

Corrosion resistance rating: 5 out of 5

Friction

Friction behavior rating: 5 out of 5

General machinability

Machinability: 60 %

Processing history

Condition: TS