PP (Polypropylene) reinforced with 40% long glass fiber.The key features are:


  • Excellent anti creeep and fatigue resistance
  • Low warpage
  • Chemical coupling
  • High strength

  • Impact modified grade

    This material data has been provided by Xiamen LFT Composite Plastic Co.,ltd.

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Properties

    General

    PropertyTemperatureValueComment

    Density

    23.0 °C

    1.12 g/cm³

    Show Supplier Material materials with Density of 1.12 g/cm³

    ASTM D792

    Mechanical

    PropertyTemperatureValueComment

    Elastic modulus

    23.0 °C

    6.9 GPa

    Show Supplier Material materials with Elastic modulus of 6.9 GPa

    ASTM D638

    Elongation

    23.0 °C

    2 - 3 %

    Show Supplier Material materials with Elongation of 2 - 3 %

    ASTM D638

    Flexural modulus

    23.0 °C

    6.34 GPa

    Show Supplier Material materials with Flexural modulus of 6.34 GPa

    ASTM D790

    Flexural strength

    23.0 °C

    165 MPa

    Show Supplier Material materials with Flexural strength of 165 MPa

    ASTM D790

    Impact strength, Izod notched, ASTM

    23.0 °C

    214 J/m

    Show Supplier Material materials with Impact strength, Izod notched, ASTM of 214 J/m

    ASTM D256

    Impact strength, Izod unnotched, ASTM

    23.0 °C

    801 J/m

    Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 801 J/m

    ASTM D4812

    Tensile strength

    23.0 °C

    121 MPa

    Show Supplier Material materials with Tensile strength of 121 MPa

    ASTM D638

    Thermal

    PropertyValueComment

    Heat deflection temperature, 1.80 MPa

    149 °C

    Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 149 °C

    ASTM D648

    Flammability

    HB ASTM D635, for 1.5mm

    Rheological Properties

    PropertyTemperatureValueComment

    Shrinkage

    23.0 °C

    0.1 - 0.3 %

    Show Supplier Material materials with Shrinkage of 0.1 - 0.3 %

    ASTM D955, (1/8 in (3.2 mm)section)

    Technological properties

    Property
    Application areas

    Power tools, Pump shell, Pipe fittings

    Fillers

    30% Long Glass Fiber

    Processing methods