Description

Common features of Hytrel® thermoplastic polyester elastomer include mechanical and physical properties such as exceptional toughness and resilience, high resistance to creep, impact and flex fatigue, flexibility at low temperatures and good retention of properties at elevated temperatures. In addition, it resists many industrial chemicals, oils and solvents. Special grades include heat stabilised, flame retardant, food contact compliant, blow molding and extrusion grades. Concentrates offered include black pigments, UV protection additives, heat stabilisers, and flame retardants. Hytrel® thermoplastic polyester elastomer is plasticiser free.The good melt stability of Hytrel® thermoplastic polyester elastomer normally enables the recycling of properly handled production waste. If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-24 kJ/g of base polymer) in appropriately equipped installations.For disposal, local regulations have to be observed. Hytrel® thermoplastic polyester elastomer typically is used in demanding applications in the automotive, fluid power, electrical/electronic, consumer goods, appliance and power tool, sporting goods, furniture, industrial and off-road transportation/equipment industry.Hytrel® PC952 NC010 is a medium modulus grade with nominal durometer hardness of 55D, contains non-discoloring stabilizer and is recommended for injection molding applications.Developed for applications such as parts for the healthcare industry.PREMIUM CONTROL for HEALTHCARE APPLICATIONSThis product is manufactured according to Good Manufacturing Practice (GMP) principles and generally accepted in food contact applications in the USA when meeting applicable use conditions. This product is also tested against ISO 10993-5 and -11 and selected parts of USP Class VI and FDA drug and device master files (DMF and MAF) have been established.For details, individual compliance statements are available from your DuPont representative.

This material data has been provided by Matmatch.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.19 g/cm³

Show Material materials with Density of 1.19 g/cm³

ISO 1183

Water absorption

23.0 °C

0.6 %

Show Material materials with Water absorption of 0.6 %

Sim. to ISO 62 | Immersion 24h

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

0.19 GPa

Show Material materials with Elastic modulus of 0.19 GPa

ISO 527-1/-2

Elongation

23.0 °C

780 %

Show Material materials with Elongation of 780 %

ISO 527-1/-2

Flexural modulus

23.0 °C

0.2 GPa

Show Material materials with Flexural modulus of 0.2 GPa

ISO 178

Hardness, Shore D

23.0 °C

55 [-]

Show Material materials with Hardness, Shore D of 55 [-]

max., ISO 7619-1

Impact strength, Charpy notched

-40.0 °C

30 kJ/m²

Show Material materials with Impact strength, Charpy notched of 30 kJ/m²

No Break @ 23°C, ISO 179/1eU

-6.0 °C

150 kJ/m²

Show Material materials with Impact strength, Charpy notched of 150 kJ/m²

No Break @ 23°C, ISO 179/1eU

Poisson's ratio

23.0 °C

0.48 [-]

Show Material materials with Poisson's ratio of 0.48 [-]

Tear strength

23.0 °C

133 kN/m

Show Material materials with Tear strength of 133 kN/m

ISO 34-1

Tear strength, transverse

23.0 °C

133 kN/m

Show Material materials with Tear strength, transverse of 133 kN/m

ISO 34-1

Tensile strength

23.0 °C

43 MPa

Show Material materials with Tensile strength of 43 MPa

ISO 527-1/-2

Impact strength, Charpy unnotched

No Break @ 23,-6°C, ISO 179/1eA

Thermal

PropertyTemperatureValueComment

Brittleness temperature

-98 °C

Show Material materials with Brittleness temperature of -98 °C

ISO 974

Coefficient of thermal expansion

23.0 °C

2E-4 1/K

Show Material materials with Coefficient of thermal expansion of 2E-4 1/K

ISO 11359-1/-2

Coefficient of thermal expansion, transverse

23.0 °C

1.9E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 1.9E-4 1/K

ISO 11359-1/-2

Glass transition temperature

-20 °C

Show Material materials with Glass transition temperature of -20 °C

ISO 11357-1/-2 | 18°F/min

Heat deflection temperature, 0.45 MPa

65 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 65 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

45 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 45 °C

ISO 75-1/-2

Melting point

203 °C

Show Material materials with Melting point of 203 °C

ISO 11357-1/-3 | 18°F/min

Specific heat capacity

23.0 °C

2110 J/(kg·K)

Show Material materials with Specific heat capacity of 2110 J/(kg·K)

of melt

Thermal diffusivity

23.0 °C

0 mm²/s

Show Material materials with Thermal diffusivity of 0 mm²/s

Vicat softening temperature

180 °C

Show Material materials with Vicat softening temperature of 180 °C

ISO 306 | 90°F, 2 lbf

Flammability

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, Oxygen index: 21 %

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Material materials with Comparative tracking index of 600 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

4.9 [-]

Show Material materials with Dielectric constant, 100Hz of 4.9 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

4.6 [-]

Show Material materials with Dielectric constant, 1MHz of 4.6 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

20 kV/mm

Show Material materials with Dielectric strength of 20 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

9E-3 [-]

Show Material materials with Dissipation factor, 100Hz of 9E-3 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.04 [-]

Show Material materials with Dissipation factor, 1MHz of 0.04 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

1.00E+15 Ω/sq

Show Material materials with Surface resistivity of 1.00E+15 Ω/sq

min. | IEC 62631-3-2

Volume resistivity

23.0 °C

4.00E+13 Ω·cm

Show Material materials with Volume resistivity of 4.00E+13 Ω·cm

IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

18 g/10min

Show Material materials with Melt mass-flow rate of 18 g/10min

ISO 1133 | 220°C/2.16kg

Melt volume-flow rate

17.5 cm³/10min

Show Material materials with Melt volume-flow rate of 17.5 cm³/10min

ISO 1133

Shrinkage

23.0 °C

1.4 %

Show Material materials with Shrinkage of 1.4 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.4 %

Show Material materials with Shrinkage, transverse of 1.4 %

ISO 294-4, 2577

Technological properties

Property
Processing methods

Drying Recommended: yes, Drying Temperature: 100°C, Drying Time, Dehumidified Dryer: 2-3h, Processing Moisture Content: ≤0.08%, Melt Temperature Optimum: 230°C, Min. melt temperature: 220°C, Max. melt temperature: 250°C, Mold Temperature Optimum: 45°C, Min. mold temperature: 45°C, Max. mold temperature: 55°C