NS106 is one of the most popular grades of nickel silver for deep drawing, spinning and other cold forming operations. It combines good strength and ductility with outstanding resistance to wear, corrosion and tarnish. It accepts a high degree of polish to a silvery white colour, aesthetically pleasing in its own right, while also providing an excellent base material for plated silverware - still one of its traditional uses. The alloy also finds many electrical and electronic applications and is readily soldered and silver brazed. The sheets are stocked in soft temper suitable for extensive cold working.

Related Standards

Equivalent Materials

This material data has been provided by Matmatch.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.75 g/cm³

Show Material materials with Density of 8.75 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

135 GPa

Show Material materials with Elastic modulus of 135 GPa

Elongation

23.0 °C

45 %

Show Material materials with Elongation of 45 %

Hardness, Vickers

23.0 °C

80 [-]

Show Material materials with Hardness, Vickers of 80 [-]

Tensile strength

23.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

Yield strength Rp0.2

23.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

Thermal

PropertyTemperatureValue

Melting point

1060 - 1110 °C

Show Material materials with Melting point of 1060 - 1110 °C

Thermal conductivity

23.0 °C

25 W/(m·K)

Show Material materials with Thermal conductivity of 25 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

23.0 °C

3.48E+6 S/m

Show Material materials with Electrical conductivity of 3.48E+6 S/m

Electrical resistivity

23.0 °C

2.9E-7 Ω·m

Show Material materials with Electrical resistivity of 2.9E-7 Ω·m

Specific Electrical conductivity

6 % IACS

Show Material materials with Specific Electrical conductivity of 6 % IACS

Magnetic

PropertyTemperatureValueComment

Relative magnetic permeability

23.0 °C

1.05 [-]

Show Material materials with Relative magnetic permeability of 1.05 [-]

max.

Chemical properties

PropertyValueComment

Copper

60 - 65 %

Show Material materials with Copper of 60 - 65 %

Iron

0.3 %

Show Material materials with Iron of 0.3 %

max.

Lead

0.03 %

Show Material materials with Lead of 0.03 %

max.

Manganese

0.05 - 0.5 %

Show Material materials with Manganese of 0.05 - 0.5 %

Nickel

17 - 19 %

Show Material materials with Nickel of 17 - 19 %

Zinc

Balance

Technological properties

Property
Application areas

General: Architectural metalwork, panels and trim, holloware, musical instruments, medals and medallions, costume jewellery, nameplates, cosmetic cases, lamp caps, lighting fittings, platters, bowls, dials, relay and contact springs, medical, industrial and scientific instrument components

Cold Forming

Very good cold working characteristics

Corrosion properties

Excellent corrosion resistance