Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 120 - 156 GPa Show Material materials with Elastic modulus of 120 - 156 GPa | Typical for Cast Copper Nickel Grade |
Elongation A50 | 23.0 °C | 25 % Show Material materials with Elongation A50 of 25 % | |
Poisson's ratio | 23.0 °C | 0.34 [-] Show Material materials with Poisson's ratio of 0.34 [-] | Typical for Cast Copper Nickel Grade |
Tensile strength | 23.0 °C | 448 MPa Show Material materials with Tensile strength of 448 MPa | |
Yield strength Rp0.5 | 23.0 °C | 241 MPa Show Material materials with Yield strength Rp0.5 of 241 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.8E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K | Typical for Cast Copper Nickel Grade |
Melting point | 1100 - 1240 °C Show Material materials with Melting point of 1100 - 1240 °C | Typical for Cast Copper Nickel Grade | |
Specific heat capacity | 23.0 °C | 377 J/(kg·K) Show Material materials with Specific heat capacity of 377 J/(kg·K) | Typical for Cast Copper Nickel Grade |
Thermal conductivity | 23.0 °C | 23 - 45 W/(m·K) Show Material materials with Thermal conductivity of 23 - 45 W/(m·K) | Typical for Cast Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Iron | 0.25 - 1.5 % Show Material materials with Iron of 0.25 - 1.5 % |
Lead | 0.01 % Show Material materials with Lead of 0.01 % |
Manganese | 1.5 % Show Material materials with Manganese of 1.5 % |
Nickel | 28 - 32 % Show Material materials with Nickel of 28 - 32 % |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % |
Sulfur | 0.02 % Show Material materials with Sulfur of 0.02 % |