Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 120 - 156 GPa Show Material materials with Elastic modulus of 120 - 156 GPa | Typical for Cast Copper Nickel Grade |
Elongation A50 | 23.0 °C | 4 % Show Material materials with Elongation A50 of 4 % | |
Hardness, Rockwell C | 23.0 °C | 32 [-] Show Material materials with Hardness, Rockwell C of 32 [-] | |
Poisson's ratio | 23.0 °C | 0.34 [-] Show Material materials with Poisson's ratio of 0.34 [-] | Typical for Cast Copper Nickel Grade |
Tensile strength | 23.0 °C | 758 MPa Show Material materials with Tensile strength of 758 MPa | |
Yield strength Rp0.5 | 23.0 °C | 724 MPa Show Material materials with Yield strength Rp0.5 of 724 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.8E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K | Typical for Cast Copper Nickel Grade |
Melting point | 1100 - 1240 °C Show Material materials with Melting point of 1100 - 1240 °C | Typical for Cast Copper Nickel Grade | |
Specific heat capacity | 23.0 °C | 377 J/(kg·K) Show Material materials with Specific heat capacity of 377 J/(kg·K) | Typical for Cast Copper Nickel Grade |
Thermal conductivity | 23.0 °C | 23 - 45 W/(m·K) Show Material materials with Thermal conductivity of 23 - 45 W/(m·K) | Typical for Cast Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Lead | 0.02 % Show Material materials with Lead of 0.02 % |
Manganese | 0.05 - 0.3 % Show Material materials with Manganese of 0.05 - 0.3 % |
Nickel | 14.5 - 15.5 % Show Material materials with Nickel of 14.5 - 15.5 % |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % |
Tin | 7.5 - 8.5 % Show Material materials with Tin of 7.5 - 8.5 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |