EN 1652 Grade CuZn20Al2As R390

Want to keep this datasheet? Save it now in your required format

Description

CuZn20Al2As (CW702R former identification: CuZn20Al2) is an unhardenable copper alloy. High hardness and strength values are achievable by cold forming only. Strength properties, corrosion resistance and oxidation resistance are increasable by Al-addition. CuZn20Al2As is seawater and dezincification resistant, and insensitive to stress corrosion in stress-relieved condition. Processing properties: warm forming: moderately cold forming: moderately machinability: moderately hard soldering: moderately soft soldering: unfavorable TIG-welding: good burnishing: very good The material is predominantly suitable for smooth and ribbed tubes and for heat-exchanger in condenser construction as well as for seawater pipelines. It is due to its favorable corrosion and erosion behaviour a reliable material in cooling water with salinities of more than 0,2%, e.g. in brack and seawater at water speed up to 2,5 m/s. In the case of a natural protective oxide film damage occurs a self-healing process.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.33 - 8.4 g/cm³

Show Material materials with Density of 8.33 - 8.4 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

110 - 112 GPa

Show Material materials with Elastic modulus of 110 - 112 GPa

50.0 °C

110 - 130 GPa

Show Material materials with Elastic modulus of 110 - 130 GPa

100.0 °C

108 - 128 GPa

Show Material materials with Elastic modulus of 108 - 128 GPa

150.0 °C

107 - 126 GPa

Show Material materials with Elastic modulus of 107 - 126 GPa

200.0 °C

106 - 123 GPa

Show Material materials with Elastic modulus of 106 - 123 GPa

250.0 °C

105 - 120 GPa

Show Material materials with Elastic modulus of 105 - 120 GPa

300.0 °C

118 GPa

Show Material materials with Elastic modulus of 118 GPa

350.0 °C

115 GPa

Show Material materials with Elastic modulus of 115 GPa

400.0 °C

112 GPa

Show Material materials with Elastic modulus of 112 GPa

450.0 °C

109 GPa

Show Material materials with Elastic modulus of 109 GPa

500.0 °C

105 GPa

Show Material materials with Elastic modulus of 105 GPa

Elongation

20.0 °C

25 - 45 %

Show Material materials with Elongation of 25 - 45 %

Elongation, transverse

20.0 °C

35 %

Show Material materials with Elongation, transverse of 35 %

Hardness, Vickers

20.0 °C

110 [-]

Show Material materials with Hardness, Vickers of 110 [-]

Shear modulus

20.0 °C

42 GPa

Show Material materials with Shear modulus of 42 GPa

Tensile strength

20.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

Tensile strength, transverse

20.0 °C

390 MPa

Show Material materials with Tensile strength, transverse of 390 MPa

Yield strength Rp0.2

10.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

20.0 °C

150 - 240 MPa

Show Material materials with Yield strength Rp0.2 of 150 - 240 MPa

50.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

100.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

150.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2 of 225 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 240 MPa

50.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 240 MPa

100.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2, transverse of 230 MPa

150.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2, transverse of 225 MPa

Unlock all property charts

Yield strength Rp1.0

20.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

50.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

100.0 °C

148 MPa

Show Material materials with Yield strength Rp1.0 of 148 MPa

150.0 °C

143 MPa

Show Material materials with Yield strength Rp1.0 of 143 MPa

200.0 °C

138 MPa

Show Material materials with Yield strength Rp1.0 of 138 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

200.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

Melting point

875 - 1075 °C

Show Material materials with Melting point of 875 - 1075 °C

Typical for Wrought Copper Brass

Specific heat capacity

20.0 °C

377 J/(kg·K)

Show Material materials with Specific heat capacity of 377 J/(kg·K)

Thermal conductivity

20.0 °C

100 W/(m·K)

Show Material materials with Thermal conductivity of 100 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

1.34E+7 S/m

Show Material materials with Electrical conductivity of 1.34E+7 S/m

Electrical resistivity

20.0 °C

7.5E-8 Ω·m

Show Material materials with Electrical resistivity of 7.5E-8 Ω·m

Chemical properties

PropertyValue

Aluminium

1.8 - 2.3 %

Show Material materials with Aluminium of 1.8 - 2.3 %

Arsenic

0.02 - 0.06 %

Show Material materials with Arsenic of 0.02 - 0.06 %

Copper

76 - 79 %

Show Material materials with Copper of 76 - 79 %

Iron

0.07 %

Show Material materials with Iron of 0.07 %

Lead

0.05 - 0.07 %

Show Material materials with Lead of 0.05 - 0.07 %

Magnesium

5E-3 %

Show Material materials with Magnesium of 5E-3 %

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

Nickel

0.1 %

Show Material materials with Nickel of 0.1 %

Phosphorus

0.01 %

Show Material materials with Phosphorus of 0.01 %