General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 8.9 g/cm³ Show Material materials with Density of 8.9 g/cm³ | Typical for Wrought Copper Pure / Low Alloyed Copper |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 95 - 98 GPa Show Material materials with Elastic modulus of 95 - 98 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Poisson's ratio | 23.0 °C | 0.34 [-] Show Material materials with Poisson's ratio of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Shear modulus | 23.0 °C | 48 GPa Show Material materials with Shear modulus of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Tensile strength | 23.0 °C | 310 MPa Show Material materials with Tensile strength of 310 MPa | |
Yield strength Rp0.5 | 23.0 °C | 275 MPa Show Material materials with Yield strength Rp0.5 of 275 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.6E-5 - 1.8E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.8E-5 1/K | Typical for Wrought Copper Pure / Low Alloyed Copper |
Melting point | 965 - 1100 °C Show Material materials with Melting point of 965 - 1100 °C | Typical for Wrought Copper Pure / Low Alloyed Copper | |
Specific heat capacity | 23.0 °C | 377 - 420 J/(kg·K) Show Material materials with Specific heat capacity of 377 - 420 J/(kg·K) | Typical for Wrought Copper Pure / Low Alloyed Copper |
Chemical properties
Property | Value |
---|---|
Antimony | 4E-4 % Show Material materials with Antimony of 4E-4 % |
Arsenic | 5E-4 % Show Material materials with Arsenic of 5E-4 % |
Chromium | 1E-4 % Show Material materials with Chromium of 1E-4 % |
Copper | 99.99 % Show Material materials with Copper of 99.99 % |
Iron | 1E-3 % Show Material materials with Iron of 1E-3 % |
Lead | 5E-4 % Show Material materials with Lead of 5E-4 % |
Manganese | 5E-5 % Show Material materials with Manganese of 5E-5 % |
Nickel | 1E-3 % Show Material materials with Nickel of 1E-3 % |
Phosphorus | 3E-4 % Show Material materials with Phosphorus of 3E-4 % |
Tin | 2E-4 % Show Material materials with Tin of 2E-4 % |
Zinc | 1E-4 % Show Material materials with Zinc of 1E-4 % |