The material according this standard is used for seamless, round tubes for heat exchangers, condensers, evaporators and desalination equipment.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.56 g/cm³

Show Material materials with Density of 8.56 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-253.0 °C

119 GPa

Show Material materials with Elastic modulus of 119 GPa

-195.0 °C

116 GPa

Show Material materials with Elastic modulus of 116 GPa

-100.0 °C

112 GPa

Show Material materials with Elastic modulus of 112 GPa

20.0 °C

108 - 110 GPa

Show Material materials with Elastic modulus of 108 - 110 GPa

50.0 °C

108 GPa

Show Material materials with Elastic modulus of 108 GPa

100.0 °C

108 GPa

Show Material materials with Elastic modulus of 108 GPa

150.0 °C

101 GPa

Show Material materials with Elastic modulus of 101 GPa

200.0 °C

94 GPa

Show Material materials with Elastic modulus of 94 GPa

250.0 °C

87 GPa

Show Material materials with Elastic modulus of 87 GPa

Elongation

20.0 °C

45 %

Show Material materials with Elongation of 45 %

Shear modulus

23.0 °C

40 GPa

Show Material materials with Shear modulus of 40 GPa

Typical for Wrought Copper Brass

Tensile strength

20.0 °C

360 MPa

Show Material materials with Tensile strength of 360 MPa

Yield strength Rp0.2

20.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

Yield strength Rp1.0

20.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

50.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

100.0 °C

144 MPa

Show Material materials with Yield strength Rp1.0 of 144 MPa

150.0 °C

140 MPa

Show Material materials with Yield strength Rp1.0 of 140 MPa

200.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.7E-5 - 2.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 2.1E-5 1/K

Typical for Wrought Copper Brass

Melting point

875 - 1075 °C

Show Material materials with Melting point of 875 - 1075 °C

Typical for Wrought Copper Brass

Specific heat capacity

23.0 °C

371 - 418 J/(kg·K)

Show Material materials with Specific heat capacity of 371 - 418 J/(kg·K)

Typical for Wrought Copper Brass

Thermal conductivity

20.0 °C

109 W/(m·K)

Show Material materials with Thermal conductivity of 109 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

1.41E+7 S/m

Show Material materials with Electrical conductivity of 1.41E+7 S/m

Specific Electrical conductivity

24 % IACS

Show Material materials with Specific Electrical conductivity of 24 % IACS

Chemical properties

PropertyValue

Arsenic

0.02 - 0.06 %

Show Material materials with Arsenic of 0.02 - 0.06 %

Copper

70 - 72.5 %

Show Material materials with Copper of 70 - 72.5 %

Iron

0.07 %

Show Material materials with Iron of 0.07 %

Lead

0.05 %

Show Material materials with Lead of 0.05 %

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

Nickel

0.1 %

Show Material materials with Nickel of 0.1 %

Phosphorus

0.01 %

Show Material materials with Phosphorus of 0.01 %

Tin

0.9 - 1.3 %

Show Material materials with Tin of 0.9 - 1.3 %