ASTM B251 Grade C17000 TD04

Alternative and trade names
Alloy 165 (C17200) Tube,Alloy 165 (C17200) Rod and Bar,Alloy 165 (C17200) Plate
Want to keep this datasheet? Save it now in your required format

Description

Alloy 165 Tube from Materion Brush Performance Alloys provides strength close to that of Alloy 25, with slightly lower beryllium content. Alloy 165 features high fatigue strength and magnetic permeability approaching unity.

Related Standards

Equivalent Materials

This material data has been provided by Materion Brush GmbH,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueTemperature

Density

8.41 - 8.8 g/cm³

Show Material materials with Density of 8.41 - 8.8 g/cm³ at 23.0 °C

23.0 °C

Dimension

PropertyValueComment

Diameter

0.76 - 356 mm

Show Material materials with Diameter of 0.76 - 356 mm

Length

610 - 91000 mm

Show Material materials with Length of 610 - 91000 mm

max.

Outside diameter

19.1 - 406 mm

Show Material materials with Outside diameter of 19.1 - 406 mm

Thickness

12.7 - 203.2 mm

Show Material materials with Thickness of 12.7 - 203.2 mm

Width

305 - 559 mm

Show Material materials with Width of 305 - 559 mm

Mechanical

PropertyValueTemperature

Elastic modulus

120 - 131 GPa

Show Material materials with Elastic modulus of 120 - 131 GPa at 23.0 °C

23.0 °C

Elongation

7.8 - 75 %

Show Material materials with Elongation of 7.8 - 75 % at 23.0 °C

23.0 °C

Tensile strength

410 - 750 MPa

Show Material materials with Tensile strength of 410 - 750 MPa at 23.0 °C

23.0 °C

Yield strength

600 MPa

Show Material materials with Yield strength of 600 MPa at 23.0 °C

23.0 °C

Yield strength Rp0.2

130 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 130 - 250 MPa at 23.0 °C

23.0 °C

Thermal

PropertyValueTemperature

Coefficient of thermal expansion

1.6E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.75E-5 1/K at 23.0 °C

23.0 °C

Melting point

870 °C

Show Material materials with Melting point of 870 °C

Specific heat capacity

410 J/(kg·K)

Show Material materials with Specific heat capacity of 410 J/(kg·K) at 23.0 °C

23.0 °C

Thermal conductivity

105 - 110 W/(m·K)

Show Material materials with Thermal conductivity of 105 - 110 W/(m·K) at 23.0 °C

23.0 °C

Electrical

PropertyValueTemperature

Electrical resistivity

5.8E-6 - 6.9E-6 Ω·m

Show Material materials with Electrical resistivity of 5.8E-6 - 6.9E-6 Ω·m at 23.0 °C

23.0 °C

Specific Electrical conductivity

25 - 30 % IACS

Show Material materials with Specific Electrical conductivity of 25 - 30 % IACS

Magnetic

PropertyValueTemperatureComment

Relative magnetic permeability

1 [-]

Show Material materials with Relative magnetic permeability of 1 [-] at 23.0 °C

23.0 °C

max.

Chemical properties

Property

Aluminium

0 - 0.2 %

Beryllium

1.6 - 1.85 %

Cobalt

0.2 %

min. Nickel + Cobalt

Copper

96.3 - 98.2 %

Balance

Iron

0 - 0.6 %

max., Nickel + Cobalt + Iron

Nickel

0.2 - 0.6 %

min. Nickel + Cobalt

Other

0 - 0.5 %

Silicon

0 - 0.2 %

Technological properties

Property
Application areas

Alloy 165 tube is used in crucial telecommunications applications including undersea instrument housings and repeater housings.,Typical applications include bushings, bearings and resistance welding components.,Typical applications include wear plates and resistance welding components.