Description

Alloy 165 rod and bar from Materion Performance Alloys provide strength close to that of Alloy 25, with slightly lower beryllium content. This alloy features high fatigue strength, good electrical and thermal conductivity, as well as resistance to wear, corrosion, galling, and stress relaxation.

Related Standards

Equivalent Materials

This material data has been provided by Materion Brush GmbH,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.41 - 8.8 g/cm³

Show Material materials with Density of 8.41 - 8.8 g/cm³

Dimension

PropertyValueComment

Diameter

0.76 - 76 mm

Show Material materials with Diameter of 0.76 - 76 mm

Length

610 - 91000 mm

Show Material materials with Length of 610 - 91000 mm

max.

Outside diameter

9.5 - 76 mm

Show Material materials with Outside diameter of 9.5 - 76 mm

Thickness

4.8 - 76 mm

Show Material materials with Thickness of 4.8 - 76 mm

Width

305 - 559 mm

Show Material materials with Width of 305 - 559 mm

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

120 - 131 GPa

Show Material materials with Elastic modulus of 120 - 131 GPa

Elongation

23.0 °C

3.8 - 30 %

Show Material materials with Elongation of 3.8 - 30 %

Tensile strength

23.0 °C

590 - 1180 MPa

Show Material materials with Tensile strength of 590 - 1180 MPa

Yield strength

23.0 °C

1010 MPa

Show Material materials with Yield strength of 1010 MPa

Yield strength Rp0.2

23.0 °C

520 - 720 MPa

Show Material materials with Yield strength Rp0.2 of 520 - 720 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.6E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.75E-5 1/K

Melting point

870 °C

Show Material materials with Melting point of 870 °C

Specific heat capacity

23.0 °C

410 J/(kg·K)

Show Material materials with Specific heat capacity of 410 J/(kg·K)

Thermal conductivity

23.0 °C

105 - 110 W/(m·K)

Show Material materials with Thermal conductivity of 105 - 110 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

5.8E-6 - 6.9E-6 Ω·m

Show Material materials with Electrical resistivity of 5.8E-6 - 6.9E-6 Ω·m

Specific Electrical conductivity

25 - 30 % IACS

Show Material materials with Specific Electrical conductivity of 25 - 30 % IACS

Magnetic

PropertyTemperatureValueComment

Relative magnetic permeability

23.0 °C

1 [-]

Show Material materials with Relative magnetic permeability of 1 [-]

max.

Chemical properties

PropertyValueComment

Aluminium

0 - 0.2 %

Show Material materials with Aluminium of 0 - 0.2 %

Beryllium

1.6 - 1.85 %

Show Material materials with Beryllium of 1.6 - 1.85 %

Cobalt

0.2 %

Show Material materials with Cobalt of 0.2 %

min. Nickel + Cobalt

Copper

96.3 - 98.2 %

Show Material materials with Copper of 96.3 - 98.2 %

Balance

Iron

0 - 0.6 %

Show Material materials with Iron of 0 - 0.6 %

max., Nickel + Cobalt + Iron

Nickel

0.2 - 0.6 %

Show Material materials with Nickel of 0.2 - 0.6 %

min. Nickel + Cobalt

Other

0 - 0.5 %

Show Material materials with Other of 0 - 0.5 %

Silicon

0 - 0.2 %

Show Material materials with Silicon of 0 - 0.2 %

Technological properties

Property
Application areas

Typical applications include bushings, bearings and resistance welding components.,Alloy 165 tube is used in crucial telecommunications applications including undersea instrument housings and repeater housings.,Typical applications include wear plates and resistance welding components.