Allgemein
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A5 | 23.0 °C | 1.5 % Show Supplier Material materials with Dehnung A5 of 1.5 % | |
Druckfestigkeit | 23.0 °C | 1310 MPa Show Supplier Material materials with Druckfestigkeit of 1310 MPa | |
Druckfestigkeit, 0,1% | 23.0 °C | 483 MPa Show Supplier Material materials with Druckfestigkeit, 0,1% of 483 MPa | |
Elastizitätsmodul | 23.0 °C | 103 GPa Show Supplier Material materials with Elastizitätsmodul of 103 GPa | |
Flächenreduzierung | 23.0 °C | 0.5 % Show Supplier Material materials with Flächenreduzierung of 0.5 % | |
Härte, HBW | 23.0 °C | 285 [-] Show Supplier Material materials with Härte, HBW of 285 [-] | HBW 10/3000 |
Härte, Rockwell C | 23.0 °C | 29 [-] Show Supplier Material materials with Härte, Rockwell C of 29 [-] | |
Izod Aufprallenergie | 23.0 °C | 2.7 J Show Supplier Material materials with Izod Aufprallenergie of 2.7 J | |
Kerbschlagenergie | 23.0 °C | 2.7 J Show Supplier Material materials with Kerbschlagenergie of 2.7 J | |
Scherfestigkeit | 23.0 °C | 448 MPa Show Supplier Material materials with Scherfestigkeit of 448 MPa | |
Streckgrenze Rp0,5 | 23.0 °C | 379 MPa Show Supplier Material materials with Streckgrenze Rp0,5 of 379 MPa | |
Zugfestigkeit | 23.0 °C | 552 MPa Show Supplier Material materials with Zugfestigkeit of 552 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.62E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.62E-5 1/K |
Spezifische Wärmekapazität | 23.0 °C | 420 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 420 J/(kg·K) |
Wärmeleitfähigkeit | 23.0 °C | 42 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 42 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 23.0 °C | 6.00E+6 S/m Show Supplier Material materials with Elektrische Leitfähigkeit of 6.00E+6 S/m |
Specific Electrical conductivity | 10 % IACS Show Supplier Material materials with Specific Electrical conductivity of 10 % IACS |
Chemical properties
Technological properties
Property | ||
---|---|---|
Application areas | AMPCO® 21 is used for guide port bushings and wear strips replacing hardened steel and for some cams when no impact is involved. However, the largest single use is as die rings, inserts, forming rolls, etc. in forming, bending or drawing operations, especially when stainless steel is the material being processed. AMPCO® 21 is also widely used as work support blades for the centerless grinding of steel rods. |