Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 56.0 % Show Supplier Material materials with Bio-based content of 56.0 % | dry | ASTM D6866-12 Method B |
Dichte | 1.05 g/cm³ Show Supplier Material materials with Dichte of 1.05 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 30 % Show Supplier Material materials with Dehnung of 30 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Dehnung of 50 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 1 GPa Show Supplier Material materials with Elastizitätsmodul of 1 GPa | conditioned | ISO 527-1/-2 | |
2 GPa Show Supplier Material materials with Elastizitätsmodul of 2 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 6 % Show Supplier Material materials with Elongation at yield of 6 % | dry | ISO 527-1/-2 | |
20 % Show Supplier Material materials with Elongation at yield of 20 % | conditioned | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 20 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 20 kJ/m² | dry | ISO 179/1eA |
23 °C | 75 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 75 kJ/m² | dry, conditioned | ISO 179/1eA | |
Zugfestigkeit | 35 MPa Show Supplier Material materials with Zugfestigkeit of 35 MPa | conditioned | ISO 527-1/-2 | |
50 MPa Show Supplier Material materials with Zugfestigkeit of 50 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schmelzpunkt | 250 °C Show Supplier Material materials with Schmelzpunkt of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Durchschlagfestigkeit | 36 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 36 kV/mm | dry | IEC 60243-1 |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzmassenflussrate | 290 °C | 28.0 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 28.0 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 290 °C | 32 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 32 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.8 % Show Supplier Material materials with Schrumpfung of 1.8 % | dry | ISO 294-4 | Normal | |
2.8 % Show Supplier Material materials with Schrumpfung of 2.8 % | dry | ISO 294-4 | Parallel |
Technological properties
Property |
---|