Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.4 g/cm³ Show Supplier Material materials with Dichte of 1.4 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 |
Wasserabsorption | 5.9 % Show Supplier Material materials with Wasserabsorption of 5.9 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 9.7 GPa Show Supplier Material materials with Biegemodul of 9.7 GPa | dry | ISO 178 | |
Dehnung | 2.7 % Show Supplier Material materials with Dehnung of 2.7 % | dry | ISO 527-1/-2 | |
6 % Show Supplier Material materials with Dehnung of 6 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 7 GPa Show Supplier Material materials with Elastizitätsmodul of 7 GPa | conditioned | ISO 527-1/-2 | |
11.5 GPa Show Supplier Material materials with Elastizitätsmodul of 11.5 GPa | dry | ISO 527-1/-2 | ||
Flexural yield strength | 255 MPa Show Supplier Material materials with Flexural yield strength of 255 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry | ISO 179/1eA |
23 °C | 18 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 18 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 70 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 70 kJ/m² | dry | ISO 179/1eU |
23 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 120 MPa Show Supplier Material materials with Zugfestigkeit of 120 MPa | conditioned | ISO 527-1/-2 | |
190 MPa Show Supplier Material materials with Zugfestigkeit of 190 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperaturleitfähigkeit | 1.1e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.1e-07 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 210 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 210 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1150 g/cm³ Show Supplier Material materials with Density of melt of 1150 g/cm³ | dry | - | |
Schrumpfung | 0.15 % Show Supplier Material materials with Schrumpfung of 0.15 % | dry | ISO 294-4 | Parallel |
1 % Show Supplier Material materials with Schrumpfung of 1 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2110 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2110 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.27 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.27 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Fillers | 35% Glass Fiber |