Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 0.76 g/cm³ Show Supplier Material materials with Dichte of 0.76 g/cm³ | dry | ISO 60 |
1.24 g/cm³ Show Supplier Material materials with Dichte of 1.24 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | dry | Sim. to ISO 62 |
Wasserabsorption | 0.6 % Show Supplier Material materials with Wasserabsorption of 0.6 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegemodul | 0.28 GPa Show Supplier Material materials with Biegemodul of 0.28 GPa | dry | ISO 178 | ||
Dehnung | 300 % Show Supplier Material materials with Dehnung of 300 % | dry | ISO 527-1/-2 | ||
680 % Show Supplier Material materials with Dehnung of 680 % | dry | ISO 527-1/-2 | |||
Elastizitätsmodul | 0.28 GPa Show Supplier Material materials with Elastizitätsmodul of 0.28 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 29.0 % Show Supplier Material materials with Elongation at yield of 29.0 % | dry | ISO 527-1/-2 | ||
Härte, Shore D | 60 [-] Show Supplier Material materials with Härte, Shore D of 60 [-] | dry | ISO 868 | 3s | |
Reißfestigkeit | 144 kN/m Show Supplier Material materials with Reißfestigkeit of 144 kN/m | dry | ISO 34-1; Method B | ||
161 kN/m Show Supplier Material materials with Reißfestigkeit of 161 kN/m | dry | ISO 34-1; Method B | |||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 12 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | dry | ISO 179/1eA | |
Zugfestigkeit | 31.5 MPa Show Supplier Material materials with Zugfestigkeit of 31.5 MPa | dry | ISO 527-1/-2 | ||
49 MPa Show Supplier Material materials with Zugfestigkeit of 49 MPa | dry | ISO 527-1/-2 | Normal |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|
Entflammbarkeit | HB | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes |
Koeffizient der thermischen Ausdehnung | 1.85e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.85e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.85e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.85e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 212 °C Show Supplier Material materials with Schmelzpunkt of 212 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Vicat-Erweichungstemperatur | 125 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 125 °C | dry | ISO 306 | 50°C/h 50N |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.4 [-] | dry | IEC 62631-2-1 | 1MHz |
3.8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.8 [-] | dry | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 22 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 22 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 110 [-] Show Supplier Material materials with Verlustfaktor of 110 [-] | dry | IEC 62631-2-1 | 100Hz |
340 [-] Show Supplier Material materials with Verlustfaktor of 340 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 4 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 4 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.5 % Show Supplier Material materials with Schrumpfung of 1.5 % | dry | Sim. to ISO 294-4 | Parallel | |
1.75 % Show Supplier Material materials with Schrumpfung of 1.75 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Application areas | Cooking Bag, Conveyor Belts, Truck Trailer Power and Signal Cord, Power transmission belts | |
Certifications | Yellow Card Available |