Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.25 g/cm³ Show Supplier Material materials with Dichte of 1.25 g/cm³ | dry | ISO 1183 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dehnung | 365 % Show Supplier Material materials with Dehnung of 365 % | dry | ISO 527-1/-2 | ||
Elastizitätsmodul | 0.43 GPa Show Supplier Material materials with Elastizitätsmodul of 0.43 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 24 % Show Supplier Material materials with Elongation at yield of 24 % | dry | ISO 527-1/-2 | ||
Härte, Shore D | 62 [-] Show Supplier Material materials with Härte, Shore D of 62 [-] | dry | ISO 868 | 3s | |
Reißfestigkeit | 150 kN/m Show Supplier Material materials with Reißfestigkeit of 150 kN/m | dry | ISO 34-1; Method B | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 7 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | dry | ISO 179/1eA | |
23 °C | 23 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 23 kJ/m² | dry | ISO 179/1eA | ||
Zugfestigkeit | 35 MPa Show Supplier Material materials with Zugfestigkeit of 35 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|
Entflammbarkeit | HB | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes |
Relative temperature index, electrical | 50 °C Show Supplier Material materials with Relative temperature index, electrical of 50 °C | dry | 2 mm | UL746B | |
Relative temperature index, mechanical impact | 50 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 50 °C | dry | 2 mm | UL746B | |
Relative temperature index, mechanical strength | 50 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 50 °C | dry | 2 mm | UL746B | |
Schmelzpunkt | 221 °C Show Supplier Material materials with Schmelzpunkt of 221 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 26 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 26 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Bed Springs | |
Certifications | Yellow Card Available |