Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.08 g/cm³ Show Supplier Material materials with Dichte of 1.08 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.9 % Show Supplier Material materials with Moisture absorption of 2.9 % | dry | Sim. to ISO 62 |
Wasserabsorption | 7.4 % Show Supplier Material materials with Wasserabsorption of 7.4 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 0.55 GPa Show Supplier Material materials with Biegemodul of 0.55 GPa | conditioned | ISO 178 | |
2.1 GPa Show Supplier Material materials with Biegemodul of 2.1 GPa | dry | ISO 178 | ||
Dehnung | -40 °C | 15 % Show Supplier Material materials with Dehnung of 15 % | dry | ISO 527-1/-2 |
50 % Show Supplier Material materials with Dehnung of 50 % | dry, conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | -40 °C | 2.5 GPa Show Supplier Material materials with Elastizitätsmodul of 2.5 GPa | dry | ISO 527-1/-2 |
0.62 GPa Show Supplier Material materials with Elastizitätsmodul of 0.62 GPa | conditioned | ISO 527-1/-2 | ||
2.2 GPa Show Supplier Material materials with Elastizitätsmodul of 2.2 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | -40 °C | 7 % Show Supplier Material materials with Elongation at yield of 7 % | dry | ISO 527-1/-2 |
4.2 % Show Supplier Material materials with Elongation at yield of 4.2 % | dry | ISO 527-1/-2 | ||
33 % Show Supplier Material materials with Elongation at yield of 33 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 23 MPa Show Supplier Material materials with Flexural yield strength of 23 MPa | conditioned | ISO 178 | |
77 MPa Show Supplier Material materials with Flexural yield strength of 77 MPa | dry | ISO 178 | ||
Puncture energy | -40 °C | 75 J Show Supplier Material materials with Puncture energy of 75 J | dry | ISO 6603-2 |
-30 °C | 64 J Show Supplier Material materials with Puncture energy of 64 J | dry | ISO 6603-2 | |
23 °C | 50 J Show Supplier Material materials with Puncture energy of 50 J | dry | ISO 6603-2 | |
Puncture force | -40 °C | 5800 N Show Supplier Material materials with Puncture force of 5800 N | dry | ISO 6603-2 |
-30 °C | 5600.0 N Show Supplier Material materials with Puncture force of 5600.0 N | dry | ISO 6603-2 | |
23 °C | 4000 N Show Supplier Material materials with Puncture force of 4000 N | dry | ISO 6603-2 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 15 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 15 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 17 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 17 kJ/m² | dry | ISO 179/1eA | |
23 °C | 60 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 60 kJ/m² | dry | ISO 179/1eA | |
Streckgrenze | -40 °C | 90 MPa Show Supplier Material materials with Streckgrenze of 90 MPa | dry | ISO 527-1/-2 |
32 MPa Show Supplier Material materials with Streckgrenze of 32 MPa | conditioned | ISO 527-1/-2 | ||
62 MPa Show Supplier Material materials with Streckgrenze of 62 MPa | dry | ISO 527-1/-2 | ||
Zugfestigkeit | -40 °C | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | dry | ISO 527-1/-2 |
47 MPa Show Supplier Material materials with Zugfestigkeit of 47 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 71 °C Show Supplier Material materials with Glasübergangstemperatur of 71 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | |
Koeffizient der thermischen Ausdehnung | 1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1e-06 1/K | dry | ISO 11359-1/-2 | Normal | |
1.5e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-06 1/K | dry | ISO 11359-1/-2 | Parallel | ||
Vicat-Erweichungstemperatur | 155 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 155 °C | dry | ISO 306 | 50°C/h 50N | |
Wärmeformbeständigkeitstemperatur | 55 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 55 °C | dry | ISO 75-1/-2 | 2 MPa | |
100 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 100 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzvolumenflussrate | 275 °C | 60 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 60 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.5 % Show Supplier Material materials with Schrumpfung of 1.5 % | dry | ISO 294-4 | Normal | |
1.6 % Show Supplier Material materials with Schrumpfung of 1.6 % | dry | ISO 294-4 | Parallel |
Technological properties
Property | ||
---|---|---|
Application areas | Outdoor power product fuel tanks |