Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.35 g/cm³ Show Supplier Material materials with Dichte of 1.35 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.9 % Show Supplier Material materials with Moisture absorption of 1.9 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.5 % Show Supplier Material materials with Wasserabsorption of 6.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.3 GPa Show Supplier Material materials with Biegemodul of 2.3 GPa | conditioned | ISO 178 | |
4.9 GPa Show Supplier Material materials with Biegemodul of 4.9 GPa | dry | ISO 178 | ||
Dehnung | 2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | |
5 % Show Supplier Material materials with Dehnung of 5 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 3.5 GPa Show Supplier Material materials with Elastizitätsmodul of 3.5 GPa | conditioned | ISO 527-1/-2 | |
6 GPa Show Supplier Material materials with Elastizitätsmodul of 6 GPa | dry | ISO 527-1/-2 | ||
Flexural yield strength | 63 MPa Show Supplier Material materials with Flexural yield strength of 63 MPa | conditioned | ISO 178 | |
124 MPa Show Supplier Material materials with Flexural yield strength of 124 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | dry | ISO 179/1eA | |
23 °C | 6 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 21 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 21 kJ/m² | dry | ISO 179/1eU |
23 °C | 21 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 21 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | 55.0 MPa Show Supplier Material materials with Zugfestigkeit of 55.0 MPa | conditioned | ISO 527-1/-2 | |
85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 3.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperaturleitfähigkeit | 1.43e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.43e-07 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 190 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 190 °C | dry | ISO 75-1/-2 | 2 MPa | |
215 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | conditioned | IEC 60243-1 | |
35 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 35 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 350 V Show Supplier Material materials with Kriechstromfestigkeit of 350 V | dry, conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 50 [-] Show Supplier Material materials with Verlustfaktor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Verlustfaktor of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Verlustfaktor of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Density of melt | 1160 g/cm³ Show Supplier Material materials with Density of melt of 1160 g/cm³ | dry | - | |
Schmelzmassenflussrate | 21 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 21 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 250 °C | 18 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 18 cm³/10min | dry | ISO 1133 |
Specific heat capacity melt | 2230 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2230 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.29 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.29 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Fuse Holders, E-Boxes | |
Fillers | 30% Glass Fiber and Glass Bead |