Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.38 g/cm³ Show Supplier Material materials with Dichte of 1.38 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.9 % Show Supplier Material materials with Moisture absorption of 1.9 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.6 % Show Supplier Material materials with Wasserabsorption of 6.6 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.2 GPa Show Supplier Material materials with Biegemodul of 2.2 GPa | conditioned | ISO 178 | |
6.1 GPa Show Supplier Material materials with Biegemodul of 6.1 GPa | dry | ISO 178 | ||
120 °C | 1.1 GPa Show Supplier Material materials with Biegemodul of 1.1 GPa | dry | ISO 178 | |
160 °C | 0.9 GPa Show Supplier Material materials with Biegemodul of 0.9 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3.7 % Show Supplier Material materials with Dehnung of 3.7 % | dry | ISO 527-1/-2 |
3.5 % Show Supplier Material materials with Dehnung of 3.5 % | dry | ISO 527-1/-2 | ||
15 % Show Supplier Material materials with Dehnung of 15 % | conditioned | ISO 527-1/-2 | ||
120 °C | 100 % Show Supplier Material materials with Dehnung of 100 % | dry | ISO 527-1/-2 | |
160 °C | 150 % Show Supplier Material materials with Dehnung of 150 % | dry | ISO 527-1/-2 | |
180 °C | 200 % Show Supplier Material materials with Dehnung of 200 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 6.3 GPa Show Supplier Material materials with Elastizitätsmodul of 6.3 GPa | dry | ISO 527-1/-2 |
3 GPa Show Supplier Material materials with Elastizitätsmodul of 3 GPa | conditioned | ISO 527-1/-2 | ||
6.1 GPa Show Supplier Material materials with Elastizitätsmodul of 6.1 GPa | dry | ISO 527-1/-2 | ||
40 °C | 5.5 GPa Show Supplier Material materials with Elastizitätsmodul of 5.5 GPa | dry | ISO 527-1/-2 | |
120 °C | 0.98 GPa Show Supplier Material materials with Elastizitätsmodul of 0.98 GPa | dry | ISO 527-1/-2 | |
160 °C | 0.72 GPa Show Supplier Material materials with Elastizitätsmodul of 0.72 GPa | dry | ISO 527-1/-2 | |
180 °C | 0.67 GPa Show Supplier Material materials with Elastizitätsmodul of 0.67 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 50 MPa Show Supplier Material materials with Flexural yield strength of 50 MPa | conditioned | ISO 178 | |
120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | ||
120 °C | 27 MPa Show Supplier Material materials with Flexural yield strength of 27 MPa | dry | ISO 178 | |
160 °C | 20 MPa Show Supplier Material materials with Flexural yield strength of 20 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 2 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 2 kJ/m² | dry | ISO 179/1eA |
-30 °C | 3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | dry | ISO 179/1eA | |
23 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | dry | ISO 179/1eU | |
23 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 100 MPa Show Supplier Material materials with Zugfestigkeit of 100 MPa | dry | ISO 527-1/-2 |
40 MPa Show Supplier Material materials with Zugfestigkeit of 40 MPa | conditioned | ISO 527-1/-2 | ||
75 MPa Show Supplier Material materials with Zugfestigkeit of 75 MPa | dry | ISO 527-1/-2 | ||
120 °C | 25 MPa Show Supplier Material materials with Zugfestigkeit of 25 MPa | dry | ISO 527-1/-2 | |
160 °C | 22 MPa Show Supplier Material materials with Zugfestigkeit of 22 MPa | dry | ISO 527-1/-2 | |
180 °C | 18 MPa Show Supplier Material materials with Zugfestigkeit of 18 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | HB | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Koeffizient der thermischen Ausdehnung | 4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | 0.71 mm | UL746B | ||
Relative temperature index, mechanical impact | 100 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 100 °C | dry | 0.71 mm | UL746B | ||
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | dry | 0.71 mm | UL746B | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperaturleitfähigkeit | 1.14e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.14e-07 mm²/s | dry | - | |||
Wärmeformbeständigkeitstemperatur | 135 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 135 °C | dry | ISO 75-1/-2 | 2 MPa | ||
205 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 205 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.2 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.2 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
15 [-] Show Supplier Material materials with Dielektrizitätskonstante of 15 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | dry, conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 50 [-] Show Supplier Material materials with Verlustfaktor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
130 [-] Show Supplier Material materials with Verlustfaktor of 130 [-] | dry | IEC 62631-2-1 | 1MHz | |
1100 [-] Show Supplier Material materials with Verlustfaktor of 1100 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3500 [-] Show Supplier Material materials with Verlustfaktor of 3500 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1160 g/cm³ Show Supplier Material materials with Density of melt of 1160 g/cm³ | dry | - | |
Schrumpfung | 0.69 % Show Supplier Material materials with Schrumpfung of 0.69 % | dry | ISO 294-4 | Normal |
0.79 % Show Supplier Material materials with Schrumpfung of 0.79 % | dry | ISO 294-4 | Parallel | |
Specific heat capacity melt | 2450 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2450 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.32 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.32 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Pulley covers | |
Certifications | Yellow Card Available | |
Fillers | 30% Mineral Powder |