Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 60 % Show Supplier Material materials with Bio-based content of 60 % | dry | ASTM D6866-12 Method B |
Dichte | 1.4 g/cm³ Show Supplier Material materials with Dichte of 1.4 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.1 % Show Supplier Material materials with Moisture absorption of 1.1 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | |
3.8 % Show Supplier Material materials with Dehnung of 3.8 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3.2 % Show Supplier Material materials with Dehnung of 3.2 % | dry | ISO 527-1/-2 | |
160 °C | 3.5 % Show Supplier Material materials with Dehnung of 3.5 % | dry | ISO 527-1/-2 | |
180 °C | 3.7 % Show Supplier Material materials with Dehnung of 3.7 % | dry | ISO 527-1/-2 | |
200 °C | 5.3 % Show Supplier Material materials with Dehnung of 5.3 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 7.7 GPa Show Supplier Material materials with Elastizitätsmodul of 7.7 GPa | conditioned | ISO 527-1/-2 | |
10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | dry | ISO 527-1/-2 | ||
120 °C | 5 GPa Show Supplier Material materials with Elastizitätsmodul of 5 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.9 GPa Show Supplier Material materials with Elastizitätsmodul of 3.9 GPa | dry | ISO 527-1/-2 | |
180 °C | 3.3 GPa Show Supplier Material materials with Elastizitätsmodul of 3.3 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.3 GPa Show Supplier Material materials with Elastizitätsmodul of 2.3 GPa | dry | ISO 527-1/-2 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 7 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | dry | ISO 179/1eA |
23 °C | 7.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7.5 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | dry | ISO 179/1eU |
23 °C | 45 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 90 MPa Show Supplier Material materials with Zugfestigkeit of 90 MPa | conditioned | ISO 527-1/-2 | |
135 MPa Show Supplier Material materials with Zugfestigkeit of 135 MPa | dry | ISO 527-1/-2 | ||
120 °C | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | dry | ISO 527-1/-2 | |
160 °C | 45 MPa Show Supplier Material materials with Zugfestigkeit of 45 MPa | dry | ISO 527-1/-2 | |
180 °C | 40 MPa Show Supplier Material materials with Zugfestigkeit of 40 MPa | dry | ISO 527-1/-2 | |
200 °C | 30 MPa Show Supplier Material materials with Zugfestigkeit of 30 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | V-0 | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Koeffizient der thermischen Ausdehnung | 4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6.6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6.6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Schmelzpunkt | 250 °C Show Supplier Material materials with Schmelzpunkt of 250 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 220 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 220 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Durchschlagfestigkeit | 30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | conditioned | IEC 60243-1 |
40 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 40 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | conditioned | IEC 60112 |
Surface resistivity | 6e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 6e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | conditioned | IEC 62631-3-1 |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Fuel System: Various Components, Fuel Vapor Separators | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |