Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.36 g/cm³ Show Supplier Material materials with Dichte of 1.36 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.6 % Show Supplier Material materials with Moisture absorption of 1.6 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6 % Show Supplier Material materials with Wasserabsorption of 6 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 6.4 GPa Show Supplier Material materials with Biegemodul of 6.4 GPa | conditioned | ISO 178 | |
9.3 GPa Show Supplier Material materials with Biegemodul of 9.3 GPa | dry | ISO 178 | ||
120 °C | 4.5 GPa Show Supplier Material materials with Biegemodul of 4.5 GPa | dry | ISO 178 | |
160 °C | 4.1 GPa Show Supplier Material materials with Biegemodul of 4.1 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3.4 % Show Supplier Material materials with Dehnung of 3.4 % | dry | ISO 527-1/-2 |
3.6 % Show Supplier Material materials with Dehnung of 3.6 % | dry | ISO 527-1/-2 | ||
6 % Show Supplier Material materials with Dehnung of 6 % | conditioned | ISO 527-1/-2 | ||
120 °C | 8 % Show Supplier Material materials with Dehnung of 8 % | dry | ISO 527-1/-2 | |
150 °C | 8.5 % Show Supplier Material materials with Dehnung of 8.5 % | dry | ISO 527-1/-2 | |
160 °C | 8.6 % Show Supplier Material materials with Dehnung of 8.6 % | dry | ISO 527-1/-2 | |
180 °C | 9 % Show Supplier Material materials with Dehnung of 9 % | dry | ISO 527-1/-2 | |
200 °C | 9.3 % Show Supplier Material materials with Dehnung of 9.3 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 10.5 GPa Show Supplier Material materials with Elastizitätsmodul of 10.5 GPa | dry | ISO 527-1/-2 |
6.5 GPa Show Supplier Material materials with Elastizitätsmodul of 6.5 GPa | conditioned | ISO 527-1/-2 | ||
10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | dry | ISO 527-1/-2 | ||
100 °C | 4.8 GPa Show Supplier Material materials with Elastizitätsmodul of 4.8 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.5 GPa Show Supplier Material materials with Elastizitätsmodul of 4.5 GPa | dry | ISO 527-1/-2 | |
150 °C | 4.1 GPa Show Supplier Material materials with Elastizitätsmodul of 4.1 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.0 GPa Show Supplier Material materials with Elastizitätsmodul of 4.0 GPa | dry | ISO 527-1/-2 | |
180 °C | 3.6 GPa Show Supplier Material materials with Elastizitätsmodul of 3.6 GPa | dry | ISO 527-1/-2 | |
200 °C | 3.4 GPa Show Supplier Material materials with Elastizitätsmodul of 3.4 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 200 MPa Show Supplier Material materials with Flexural yield strength of 200 MPa | conditioned | ISO 178 | |
295 MPa Show Supplier Material materials with Flexural yield strength of 295 MPa | dry | ISO 178 | ||
120 °C | 135 MPa Show Supplier Material materials with Flexural yield strength of 135 MPa | dry | ISO 178 | |
160 °C | 115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 10 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 13 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 13 kJ/m² | dry | ISO 179/1eA | |
23 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 65 kJ/m² | dry | ISO 179/1eU |
-30 °C | 68 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 68 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 81 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 81 kJ/m² | dry | ISO 179/1eU | |
23 °C | 88 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 88 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 250 MPa Show Supplier Material materials with Zugfestigkeit of 250 MPa | dry | ISO 527-1/-2 |
125 MPa Show Supplier Material materials with Zugfestigkeit of 125 MPa | conditioned | ISO 527-1/-2 | ||
205 MPa Show Supplier Material materials with Zugfestigkeit of 205 MPa | dry | ISO 527-1/-2 | ||
100 °C | 111 MPa Show Supplier Material materials with Zugfestigkeit of 111 MPa | dry | ISO 527-1/-2 | |
120 °C | 103 MPa Show Supplier Material materials with Zugfestigkeit of 103 MPa | dry | ISO 527-1/-2 | |
150 °C | 91 MPa Show Supplier Material materials with Zugfestigkeit of 91 MPa | dry | ISO 527-1/-2 | |
160 °C | 87 MPa Show Supplier Material materials with Zugfestigkeit of 87 MPa | dry | ISO 527-1/-2 | |
180 °C | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | dry | ISO 527-1/-2 | |
200 °C | 72 MPa Show Supplier Material materials with Zugfestigkeit of 72 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
7e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.71 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.71 mm | ||
Schmelzpunkt | 260 °C Show Supplier Material materials with Schmelzpunkt of 260 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 250 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 250 °C | dry | ISO 75-1/-2 | 2 MPa | ||
260 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 260 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 62631-2-1 | 1MHz |
3.8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.8 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.1 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.1 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
10 [-] Show Supplier Material materials with Dielektrizitätskonstante of 10 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | dry, conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 90 [-] Show Supplier Material materials with Verlustfaktor of 90 [-] | dry | IEC 62631-2-1 | 100Hz |
160 [-] Show Supplier Material materials with Verlustfaktor of 160 [-] | dry | IEC 62631-2-1 | 1MHz | |
800 [-] Show Supplier Material materials with Verlustfaktor of 800 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
2800 [-] Show Supplier Material materials with Verlustfaktor of 2800 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzmassenflussrate | 275 °C | 15.3 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 15.3 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 275 °C | 12.7 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 12.7 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 0.2 % Show Supplier Material materials with Schrumpfung of 0.2 % | dry | Sim. to ISO 294-4 | Parallel | |
1 % Show Supplier Material materials with Schrumpfung of 1 % | dry | Sim. to ISO 294-4 | Normal | ||
Specific heat capacity melt | 2170 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2170 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.28 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.28 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Air inlet manifolds, Integrated Air Inlet Manifolds (up to 180°C), Coolant expansion tank, Radiator end tanks | |
Fillers | 30% Glass Fiber |