Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.24 g/cm³ Show Supplier Material materials with Dichte of 1.24 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.4 % Show Supplier Material materials with Moisture absorption of 0.4 % | dry | Sim. to ISO 62 |
Wasserabsorption | 2.5 % Show Supplier Material materials with Wasserabsorption of 2.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dehnung | 300 % Show Supplier Material materials with Dehnung of 300 % | dry | ISO 527-1/-2 | ||
400 % Show Supplier Material materials with Dehnung of 400 % | dry | ISO 527-1/-2 | |||
Elastizitätsmodul | 0.21 GPa Show Supplier Material materials with Elastizitätsmodul of 0.21 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 35 % Show Supplier Material materials with Elongation at yield of 35 % | dry | ISO 527-1/-2 | ||
Härte, Shore D | 53 [-] Show Supplier Material materials with Härte, Shore D of 53 [-] | dry | ISO 868 | 3s | |
Reißfestigkeit | 125 kN/m Show Supplier Material materials with Reißfestigkeit of 125 kN/m | dry | ISO 34-1; Method B | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | dry | ISO 179/1eA | |
Zugfestigkeit | 31 MPa Show Supplier Material materials with Zugfestigkeit of 31 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 218 °C Show Supplier Material materials with Schmelzpunkt of 218 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Vicat-Erweichungstemperatur | 105 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 105 °C | dry | ISO 306 | 50°C/h 50N | |
Wärmeformbeständigkeitstemperatur | 100 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 100 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
Durchschlagfestigkeit | 21 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 21 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 400 [-] Show Supplier Material materials with Verlustfaktor of 400 [-] | dry | IEC 62631-2-1 | 1MHz |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 15 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 15 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.7 % Show Supplier Material materials with Schrumpfung of 1.7 % | dry | Sim. to ISO 294-4 | Parallel | |
1.8 % Show Supplier Material materials with Schrumpfung of 1.8 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Application areas | Railway Pads |