Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.2 g/cm³ Show Supplier Material materials with Dichte of 1.2 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | dry | Sim. to ISO 62 |
Wasserabsorption | 0.65 % Show Supplier Material materials with Wasserabsorption of 0.65 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | dry | ISO 527-1/-2 | ||
300 % Show Supplier Material materials with Dehnung of 300 % | dry | ISO 527-1/-2 | |||
Elastizitätsmodul | 0.17 GPa Show Supplier Material materials with Elastizitätsmodul of 0.17 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 33 % Show Supplier Material materials with Elongation at yield of 33 % | dry | ISO 527-1/-2 | ||
Härte, Shore D | 54 [-] Show Supplier Material materials with Härte, Shore D of 54 [-] | dry | ISO 868 | 3s | |
Reißfestigkeit | 150 kN/m Show Supplier Material materials with Reißfestigkeit of 150 kN/m | dry | ISO 34-1; Method B | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 25 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 25 kJ/m² | dry | ISO 179/1eA | |
Zugfestigkeit | 32 MPa Show Supplier Material materials with Zugfestigkeit of 32 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Glasübergangstemperatur | -64 °C Show Supplier Material materials with Glasübergangstemperatur of -64 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Koeffizient der thermischen Ausdehnung | 2e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2e-06 1/K | dry | ISO 11359-1/-2 | Parallel | ||
2e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2e-06 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 50 °C Show Supplier Material materials with Relative temperature index, electrical of 50 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical impact | 50 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 50 °C | dry | UL746B | 2 mm | ||
Relative temperature index, mechanical strength | 50 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 50 °C | dry | UL746B | 2 mm | ||
Schmelzpunkt | 204 °C Show Supplier Material materials with Schmelzpunkt of 204 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Vicat-Erweichungstemperatur | 90 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 90 °C | dry | ISO 306 | 50°C/h 50N | ||
Wärmeformbeständigkeitstemperatur | 110 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 110 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.4 [-] | dry | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 21 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 21 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 400 [-] Show Supplier Material materials with Verlustfaktor of 400 [-] | dry | IEC 62631-2-1 | 1MHz |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 23 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 23 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.55 % Show Supplier Material materials with Schrumpfung of 1.55 % | dry | Sim. to ISO 294-4 | Parallel | |
1.55 % Show Supplier Material materials with Schrumpfung of 1.55 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property |
---|