Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.37 g/cm³ Show Supplier Material materials with Dichte of 1.37 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.9 % Show Supplier Material materials with Moisture absorption of 1.9 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.5 % Show Supplier Material materials with Wasserabsorption of 6.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 2.5 % Show Supplier Material materials with Dehnung of 2.5 % | dry | ISO 527-1/-2 | |
12 % Show Supplier Material materials with Dehnung of 12 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 3.2 GPa Show Supplier Material materials with Elastizitätsmodul of 3.2 GPa | conditioned | ISO 527-1/-2 | |
7.5 GPa Show Supplier Material materials with Elastizitätsmodul of 7.5 GPa | dry | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | dry | ISO 179/1eA | |
23 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 35 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 35 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 40 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 40 kJ/m² | dry | ISO 179/1eU | |
23 °C | 45 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 50 MPa Show Supplier Material materials with Zugfestigkeit of 50 MPa | conditioned | ISO 527-1/-2 | |
110 MPa Show Supplier Material materials with Zugfestigkeit of 110 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 3.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperaturleitfähigkeit | 1.46e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.46e-07 mm²/s | dry | - | |||
Wärmeformbeständigkeitstemperatur | 180 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 180 °C | dry | ISO 75-1/-2 | 2 MPa | ||
210 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 210 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | conditioned | IEC 60243-1 | |
35 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 35 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 50 [-] Show Supplier Material materials with Verlustfaktor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
140 [-] Show Supplier Material materials with Verlustfaktor of 140 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3200 [-] Show Supplier Material materials with Verlustfaktor of 3200 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 976 g/cm³ Show Supplier Material materials with Density of melt of 976 g/cm³ | dry | - | |
Schrumpfung | 0.3 % Show Supplier Material materials with Schrumpfung of 0.3 % | dry | ISO 294-4 | Parallel |
0.9 % Show Supplier Material materials with Schrumpfung of 0.9 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2180 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2180 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.31 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.31 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Engine Cover with Air Inlet Filters, Engine Covers | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber and Mineral Powder |