Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.35 g/cm³ Show Supplier Material materials with Dichte of 1.35 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.8 % Show Supplier Material materials with Moisture absorption of 2.8 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 2.85 % Show Supplier Material materials with Wasserabsorption of 2.85 % | dry | ISO 62 | at 23°C after 24h |
10.1 % Show Supplier Material materials with Wasserabsorption of 10.1 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 8.4 GPa Show Supplier Material materials with Biegemodul of 8.4 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3.3 % Show Supplier Material materials with Dehnung of 3.3 % | dry | ISO 527-1/-2 |
3.3 % Show Supplier Material materials with Dehnung of 3.3 % | dry | ISO 527-1/-2 | ||
120 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
150 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
180 °C | 7 % Show Supplier Material materials with Dehnung of 7 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 9.3 GPa Show Supplier Material materials with Elastizitätsmodul of 9.3 GPa | dry | ISO 527-1/-2 |
9 GPa Show Supplier Material materials with Elastizitätsmodul of 9 GPa | dry | ISO 527-1/-2 | ||
65 °C | 7.3 GPa Show Supplier Material materials with Elastizitätsmodul of 7.3 GPa | dry | ISO 527-1/-2 | |
90 °C | 5.2 GPa Show Supplier Material materials with Elastizitätsmodul of 5.2 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.7 GPa Show Supplier Material materials with Elastizitätsmodul of 4.7 GPa | dry | ISO 527-1/-2 | |
150 °C | 4.5 GPa Show Supplier Material materials with Elastizitätsmodul of 4.5 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.3 GPa Show Supplier Material materials with Elastizitätsmodul of 4.3 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 9.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9.5 kJ/m² | dry | ISO 179/1eA |
Zugfestigkeit | -40 °C | 220 MPa Show Supplier Material materials with Zugfestigkeit of 220 MPa | dry | ISO 527-1/-2 |
190 MPa Show Supplier Material materials with Zugfestigkeit of 190 MPa | dry | ISO 527-1/-2 | ||
120 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | dry | ISO 527-1/-2 | |
150 °C | 95 MPa Show Supplier Material materials with Zugfestigkeit of 95 MPa | dry | ISO 527-1/-2 | |
180 °C | 88 MPa Show Supplier Material materials with Zugfestigkeit of 88 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 3e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 280 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 280 °C | dry | ISO 75-1/-2 | 2 MPa |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schrumpfung | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | dry | ISO 294-4 | Parallel |
1.3 % Show Supplier Material materials with Schrumpfung of 1.3 % | dry | ISO 294-4 | Normal | |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Fillers | 25% Glass Fiber |