Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Coefficient of friction, kinetic | 1.2 [-] Show Supplier Material materials with Coefficient of friction, kinetic of 1.2 [-] | dry | ISO 8295 |
Coefficient of friction, static | 1.5 [-] Show Supplier Material materials with Coefficient of friction, static of 1.5 [-] | dry | ISO 8295 |
Dichte | 1.13 g/cm³ Show Supplier Material materials with Dichte of 1.13 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.5 % Show Supplier Material materials with Moisture absorption of 2.5 % | dry | Sim. to ISO 62 |
Wasserabsorption | 9.5 % Show Supplier Material materials with Wasserabsorption of 9.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegemodul | 2.6 GPa Show Supplier Material materials with Biegemodul of 2.6 GPa | dry | ISO 178 | ||
Dehnung | 350 % Show Supplier Material materials with Dehnung of 350 % | dry | ISO 527-3 | Parallel | |
Elastizitätsmodul | 0.46 GPa Show Supplier Material materials with Elastizitätsmodul of 0.46 GPa | dry | DSM-Method, 50 mm/min | ||
2.9 GPa Show Supplier Material materials with Elastizitätsmodul of 2.9 GPa | dry | ISO 527-1/-2 | |||
Flexural yield strength | 90 MPa Show Supplier Material materials with Flexural yield strength of 90 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | 23 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | dry | ISO 179/1eA | |
Streckgrenze | 32 MPa Show Supplier Material materials with Streckgrenze of 32 MPa | dry | ISO 527-3 | Parallel | |
80 MPa Show Supplier Material materials with Streckgrenze of 80 MPa | dry | ISO 527-1/-2 | |||
Zugfestigkeit | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | dry | ISO 527-3 | Parallel |
Thermisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Parallel |
1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1e-06 1/K | dry | ISO 11359-1/-2 | Normal | |
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min |
Spezifische Wärmekapazität | 1550 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 1550 J/(kg·K) | dry | - | |
2250 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 2250 J/(kg·K) | dry |
Optisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Transparenz | 83 | dry | DSM method |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Melt viscosity | 260 °C | 410 Pa·s Show Supplier Material materials with Melt viscosity of 410 Pa·s | dry | DSM method, 260 °C |
Viscosity number | 168 cm³/gr Show Supplier Material materials with Viscosity number of 168 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property |
---|