Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.37 g/cm³ Show Supplier Material materials with Dichte of 1.37 g/cm³ | dry | ISO 1183 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 7 GPa Show Supplier Material materials with Biegemodul of 7 GPa | dry | ISO 178 | |
Dehnung | 2.7 % Show Supplier Material materials with Dehnung of 2.7 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 7.7 GPa Show Supplier Material materials with Elastizitätsmodul of 7.7 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 6.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6.5 kJ/m² | dry | ISO 179/1eA |
Zugfestigkeit | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 276 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 276 °C | dry | ISO 75-1/-2 | 2 MPa | |
284 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 284 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 60250 | 1GHz |
Durchschlagfestigkeit | 30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 575 V Show Supplier Material materials with Kriechstromfestigkeit of 575 V | dry | IEC 60112 | |
Verlustfaktor | 100 [-] Show Supplier Material materials with Verlustfaktor of 100 [-] | dry | IEC 60250 | 1GHz |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schrumpfung | 0.4 % Show Supplier Material materials with Schrumpfung of 0.4 % | dry | ISO 294-4 | Parallel |
1.5 % Show Supplier Material materials with Schrumpfung of 1.5 % | dry | ISO 294-4 | Normal | |
Spiral flow length | 165 | dry | - | 1.0 mm 800 bar |
180 | dry | - | 1.0 mm 900 bar | |
200 | dry | - | 1.0 mm 1000 bar |
Technological properties
Property | ||
---|---|---|
Application areas | USB-C Connectors | |
Certifications | Yellow Card Available | |
Fillers | 20% Glass Fiber |