Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.29 g/cm³ Show Supplier Material materials with Dichte of 1.29 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 3.15 % Show Supplier Material materials with Moisture absorption of 3.15 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 3.2 % Show Supplier Material materials with Wasserabsorption of 3.2 % | dry | ISO 62 | at 23°C after 24h |
11.5 % Show Supplier Material materials with Wasserabsorption of 11.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.8 GPa Show Supplier Material materials with Biegemodul of 2.8 GPa | conditioned | ISO 178 | |
5.8 GPa Show Supplier Material materials with Biegemodul of 5.8 GPa | dry | ISO 178 | ||
120 °C | 2.7 GPa Show Supplier Material materials with Biegemodul of 2.7 GPa | dry | ISO 178 | |
160 °C | 2.6 GPa Show Supplier Material materials with Biegemodul of 2.6 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | dry | ISO 527-1/-2 |
3.5 % Show Supplier Material materials with Dehnung of 3.5 % | dry | ISO 527-1/-2 | ||
12 % Show Supplier Material materials with Dehnung of 12 % | conditioned | ISO 527-1/-2 | ||
120 °C | 13 % Show Supplier Material materials with Dehnung of 13 % | dry | ISO 527-1/-2 | |
140 °C | 13 % Show Supplier Material materials with Dehnung of 13 % | dry | ISO 527-1/-2 | |
150 °C | 13 % Show Supplier Material materials with Dehnung of 13 % | dry | ISO 527-1/-2 | |
160 °C | 12 % Show Supplier Material materials with Dehnung of 12 % | dry | ISO 527-1/-2 | |
180 °C | 12 % Show Supplier Material materials with Dehnung of 12 % | dry | ISO 527-1/-2 | |
200 °C | 12 % Show Supplier Material materials with Dehnung of 12 % | dry | ISO 527-1/-2 | |
210 °C | 0.01 % Show Supplier Material materials with Dehnung of 0.01 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 6.2 GPa Show Supplier Material materials with Elastizitätsmodul of 6.2 GPa | dry | ISO 527-1/-2 |
2.8 GPa Show Supplier Material materials with Elastizitätsmodul of 2.8 GPa | conditioned | ISO 527-1/-2 | ||
6.1 GPa Show Supplier Material materials with Elastizitätsmodul of 6.1 GPa | dry | ISO 527-1/-2 | ||
100 °C | 3.1 GPa Show Supplier Material materials with Elastizitätsmodul of 3.1 GPa | dry | ISO 527-1/-2 | |
120 °C | 3 GPa Show Supplier Material materials with Elastizitätsmodul of 3 GPa | dry | ISO 527-1/-2 | |
140 °C | 2.8 GPa Show Supplier Material materials with Elastizitätsmodul of 2.8 GPa | dry | ISO 527-1/-2 | |
150 °C | 2.7 GPa Show Supplier Material materials with Elastizitätsmodul of 2.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 2.6 GPa Show Supplier Material materials with Elastizitätsmodul of 2.6 GPa | dry | ISO 527-1/-2 | |
180 °C | 2.5 GPa Show Supplier Material materials with Elastizitätsmodul of 2.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.4 GPa Show Supplier Material materials with Elastizitätsmodul of 2.4 GPa | dry | ISO 527-1/-2 | |
210 °C | 2.2 GPa Show Supplier Material materials with Elastizitätsmodul of 2.2 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 125 MPa Show Supplier Material materials with Flexural yield strength of 125 MPa | conditioned | ISO 178 | |
235 MPa Show Supplier Material materials with Flexural yield strength of 235 MPa | dry | ISO 178 | ||
120 °C | 80 MPa Show Supplier Material materials with Flexural yield strength of 80 MPa | dry | ISO 178 | |
160 °C | 75 MPa Show Supplier Material materials with Flexural yield strength of 75 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 6 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 6 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 6 kJ/m² | dry | ISO 179/1eA | |
23 °C | 13 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 13 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 45 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 45 kJ/m² | dry | ISO 179/1eU |
-30 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 100 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 155 MPa Show Supplier Material materials with Zugfestigkeit of 155 MPa | dry | ISO 527-1/-2 |
85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | conditioned | ISO 527-1/-2 | ||
140 MPa Show Supplier Material materials with Zugfestigkeit of 140 MPa | dry | ISO 527-1/-2 | ||
100 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
120 °C | 82 MPa Show Supplier Material materials with Zugfestigkeit of 82 MPa | dry | ISO 527-1/-2 | |
140 °C | 78 MPa Show Supplier Material materials with Zugfestigkeit of 78 MPa | dry | ISO 527-1/-2 | |
150 °C | 76 MPa Show Supplier Material materials with Zugfestigkeit of 76 MPa | dry | ISO 527-1/-2 | |
160 °C | 74 MPa Show Supplier Material materials with Zugfestigkeit of 74 MPa | dry | ISO 527-1/-2 | |
180 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 | |
200 °C | 66 MPa Show Supplier Material materials with Zugfestigkeit of 66 MPa | dry | ISO 527-1/-2 | |
210 °C | 64 MPa Show Supplier Material materials with Zugfestigkeit of 64 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | HB | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Koeffizient der thermischen Ausdehnung | 5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | 2 mm | UL746B | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | 2 mm | UL746B | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | 2 mm | UL746B | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperaturleitfähigkeit | 9.37e-08 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 9.37e-08 mm²/s | dry | - | |||
Vicat-Erweichungstemperatur | 290 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 290 °C | dry | ISO 306 | 50°C/h 50N | ||
Wärmeformbeständigkeitstemperatur | 275 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 275 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Kriechstromfestigkeit | 400 V Show Supplier Material materials with Kriechstromfestigkeit of 400 V | dry | IEC 60112 |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+07 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+07 Ω·cm | conditioned | IEC 62631-3-1 |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1100 g/cm³ Show Supplier Material materials with Density of melt of 1100 g/cm³ | dry | - | |
Schrumpfung | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | dry | ISO 294-4 | Parallel |
1.2 % Show Supplier Material materials with Schrumpfung of 1.2 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2540 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2540 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.267 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.267 W/(m·K) | dry | - | |
Viscosity number | 150 cm³/gr Show Supplier Material materials with Viscosity number of 150 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Chain Tensioners, Variator Roller Cover, Transmission Control Gears, Bike Body Plugs, Oil Pump Gears (2-wheelers), Automotive Connectors, Electric parking brakes, Electric brake boosters, Seat actuators, Mirror actuators, Trunk actuators, Door handle actuators, Sunroof actuators, Steering wheel adjusters | |
Certifications | Yellow Card Available | |
Fillers | 15% Glass Fiber |