Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.37 g/cm³ Show Supplier Material materials with Dichte of 1.37 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2 % Show Supplier Material materials with Moisture absorption of 2 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 2.1 % Show Supplier Material materials with Wasserabsorption of 2.1 % | dry | ISO 62 | at 23°C after 24h |
7.5 % Show Supplier Material materials with Wasserabsorption of 7.5 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 2.5 GPa Show Supplier Material materials with Biegemodul of 2.5 GPa | dry | ISO 178 | |
Dehnung | 20 % Show Supplier Material materials with Dehnung of 20 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Dehnung of 50 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 1.2 GPa Show Supplier Material materials with Elastizitätsmodul of 1.2 GPa | conditioned | ISO 527-1/-2 | |
3 GPa Show Supplier Material materials with Elastizitätsmodul of 3 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 4 % Show Supplier Material materials with Elongation at yield of 4 % | dry | ISO 527-1/-2 | |
15 % Show Supplier Material materials with Elongation at yield of 15 % | conditioned | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | dry | ISO 179/1eA | |
23 °C | 14.0 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 14.0 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | dry | ISO 179/1eU |
-30 °C | 95 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 95 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | dry | ISO 179/1eU |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | V-0 | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 3 mm | IEC 60695-2-12 | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | 0.75 mm | IEC 60695-2-12 | |||
Glow Wire Ignition Temperature | 775 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 775 °C | dry | 3 mm | IEC 60695-2-13 | ||
925 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 925 °C | dry | 0.75 mm | IEC 60695-2-13 | |||
Koeffizient der thermischen Ausdehnung | 9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | 0.75 mm | UL746B | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | 0.75 mm | UL746B | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 160 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 160 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Durchschlagfestigkeit | 20 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 20 kV/mm | conditioned | IEC 60243-1 |
25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | dry | IEC 60243-1 | |
Volume resistivity | 2e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+10 Ω·cm | conditioned | IEC 62631-3-1 |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available |