Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.16 g/cm³ Show Supplier Material materials with Dichte of 1.16 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.4 % Show Supplier Material materials with Moisture absorption of 0.4 % | dry | Sim. to ISO 62 |
Wasserabsorption | 7 % Show Supplier Material materials with Wasserabsorption of 7 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dehnung | 155 % Show Supplier Material materials with Dehnung of 155 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 0.04 GPa Show Supplier Material materials with Elastizitätsmodul of 0.04 GPa | dry | ISO 527-1/-2 | |
Härte, Shore D | 32 [-] Show Supplier Material materials with Härte, Shore D of 32 [-] | dry | ISO 868 | 3s |
Reißfestigkeit | 52 kN/m Show Supplier Material materials with Reißfestigkeit of 52 kN/m | dry | ISO 34-1; Method B | |
Zugfestigkeit | 12.5 MPa Show Supplier Material materials with Zugfestigkeit of 12.5 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.5e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-06 1/K | dry | ISO 11359-1/-2 | Parallel |
1.5e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-06 1/K | dry | ISO 11359-1/-2 | Normal | |
Schmelzpunkt | 212 °C Show Supplier Material materials with Schmelzpunkt of 212 °C | dry | ISO 11357-1/-3 | 10°C/min |
Vicat-Erweichungstemperatur | 120 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 120 °C | dry | ISO 306 | 50°C/h 50N |
127 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 127 °C | dry | ISO 306 | 50°C/h 10N |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4.4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.7 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.7 [-] | dry | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 20 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 20 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Verlustfaktor | 310 [-] Show Supplier Material materials with Verlustfaktor of 310 [-] | dry | IEC 62631-2-1 | 100Hz |
810 [-] Show Supplier Material materials with Verlustfaktor of 810 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 4.7 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 4.7 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Infusion Membrane Bags, Breathable Films for Food Packaging, Mandrels as Supportive Tool, Industrial Cords and Ropes, House Wrap | |