Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.55 g/cm³ Show Supplier Material materials with Dichte of 1.55 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.05 % Show Supplier Material materials with Moisture absorption of 0.05 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 0.05 % Show Supplier Material materials with Wasserabsorption of 0.05 % | dry | ISO 62 | at 23°C after 24h |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 11 GPa Show Supplier Material materials with Biegemodul of 11 GPa | dry | ISO 178 | |
120 °C | 5.3 GPa Show Supplier Material materials with Biegemodul of 5.3 GPa | dry | ISO 178 | |
160 °C | 4.2 GPa Show Supplier Material materials with Biegemodul of 4.2 GPa | dry | ISO 178 | |
200 °C | 3.5 GPa Show Supplier Material materials with Biegemodul of 3.5 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 |
2.1 % Show Supplier Material materials with Dehnung of 2.1 % | dry | ISO 527-1/-2 | ||
120 °C | 3.5 % Show Supplier Material materials with Dehnung of 3.5 % | dry | ISO 527-1/-2 | |
160 °C | 5 % Show Supplier Material materials with Dehnung of 5 % | dry | ISO 527-1/-2 | |
200 °C | 5.4 % Show Supplier Material materials with Dehnung of 5.4 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 12.3 GPa Show Supplier Material materials with Elastizitätsmodul of 12.3 GPa | dry | ISO 527-1/-2 |
11.5 GPa Show Supplier Material materials with Elastizitätsmodul of 11.5 GPa | dry | ISO 527-1/-2 | ||
120 °C | 5.6 GPa Show Supplier Material materials with Elastizitätsmodul of 5.6 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.6 GPa Show Supplier Material materials with Elastizitätsmodul of 3.6 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.8 GPa Show Supplier Material materials with Elastizitätsmodul of 2.8 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 225 MPa Show Supplier Material materials with Flexural yield strength of 225 MPa | dry | ISO 178 | |
120 °C | 115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | dry | ISO 178 | |
160 °C | 80 MPa Show Supplier Material materials with Flexural yield strength of 80 MPa | dry | ISO 178 | |
200 °C | 75 MPa Show Supplier Material materials with Flexural yield strength of 75 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | dry | ISO 179/1eA |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | dry | ISO 179/1eU |
Zugfestigkeit | -40 °C | 200 MPa Show Supplier Material materials with Zugfestigkeit of 200 MPa | dry | ISO 527-1/-2 |
175 MPa Show Supplier Material materials with Zugfestigkeit of 175 MPa | dry | ISO 527-1/-2 | ||
120 °C | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | dry | ISO 527-1/-2 | |
160 °C | 65 MPa Show Supplier Material materials with Zugfestigkeit of 65 MPa | dry | ISO 527-1/-2 | |
200 °C | 55.0 MPa Show Supplier Material materials with Zugfestigkeit of 55.0 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 90 °C Show Supplier Material materials with Glasübergangstemperatur of 90 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 1.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.8e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | ||
5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
1.2e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.2e-06 1/K | dry | ISO 11359-1/-2 | normal, above Tg | ||
Schmelzpunkt | 280 °C Show Supplier Material materials with Schmelzpunkt of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 265 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 265 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.7 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.7 [-] | dry | IEC 62631-2-1 | 1MHz |
Verlustfaktor | 30 [-] Show Supplier Material materials with Verlustfaktor of 30 [-] | dry | IEC 62631-2-1 | 1MHz |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Pipe Fittings | |
Certifications | Food Contact, Drinking Water | |
Fillers | 30% Glass Fiber |