Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.65 g/cm³ Show Supplier Material materials with Dichte of 1.65 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.04 % Show Supplier Material materials with Moisture absorption of 0.04 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 0.04 % Show Supplier Material materials with Wasserabsorption of 0.04 % | dry | ISO 62 | at 23°C after 24h |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 14 GPa Show Supplier Material materials with Biegemodul of 14 GPa | dry | ISO 178 | |
120 °C | 8.2 GPa Show Supplier Material materials with Biegemodul of 8.2 GPa | dry | ISO 178 | |
160 °C | 5 GPa Show Supplier Material materials with Biegemodul of 5 GPa | dry | ISO 178 | |
200 °C | 4.3 GPa Show Supplier Material materials with Biegemodul of 4.3 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Dehnung of 2 % | dry | ISO 527-1/-2 | ||
120 °C | 2.9 % Show Supplier Material materials with Dehnung of 2.9 % | dry | ISO 527-1/-2 | |
160 °C | 3.8 % Show Supplier Material materials with Dehnung of 3.8 % | dry | ISO 527-1/-2 | |
200 °C | 3.9 % Show Supplier Material materials with Dehnung of 3.9 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 17 GPa Show Supplier Material materials with Elastizitätsmodul of 17 GPa | dry | ISO 527-1/-2 |
15 GPa Show Supplier Material materials with Elastizitätsmodul of 15 GPa | dry | ISO 527-1/-2 | ||
120 °C | 9.5 GPa Show Supplier Material materials with Elastizitätsmodul of 9.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 5.3 GPa Show Supplier Material materials with Elastizitätsmodul of 5.3 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.1 GPa Show Supplier Material materials with Elastizitätsmodul of 4.1 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | |
120 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |
160 °C | 95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | |
200 °C | 70 MPa Show Supplier Material materials with Flexural yield strength of 70 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry | ISO 179/1eA |
23 °C | 10.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10.5 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 62 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 62 kJ/m² | dry | ISO 179/1eU |
23 °C | 60 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 60 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 235 MPa Show Supplier Material materials with Zugfestigkeit of 235 MPa | dry | ISO 527-1/-2 |
200 MPa Show Supplier Material materials with Zugfestigkeit of 200 MPa | dry | ISO 527-1/-2 | ||
120 °C | 100 MPa Show Supplier Material materials with Zugfestigkeit of 100 MPa | dry | ISO 527-1/-2 | |
160 °C | 65 MPa Show Supplier Material materials with Zugfestigkeit of 65 MPa | dry | ISO 527-1/-2 | |
200 °C | 50 MPa Show Supplier Material materials with Zugfestigkeit of 50 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Glasübergangstemperatur | 90 °C Show Supplier Material materials with Glasübergangstemperatur of 90 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Koeffizient der thermischen Ausdehnung | 1.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.5e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | |||
4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
1.1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.1e-06 1/K | dry | ISO 11359-1/-2 | normal, above Tg | |||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.4 mm | ||
Schmelzpunkt | 280 °C Show Supplier Material materials with Schmelzpunkt of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 265 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 265 °C | dry | ISO 75-1/-2 | 2 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 60250 | 1GHz |
4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 60250 | 5GHz | |
Durchschlagfestigkeit | 22 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 22 kV/mm | dry | IEC 60234 | |
Kriechstromfestigkeit | 150 V Show Supplier Material materials with Kriechstromfestigkeit of 150 V | dry | IEC 60112 | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | |
Verlustfaktor | 35 [-] Show Supplier Material materials with Verlustfaktor of 35 [-] | dry | IEC 60250 | 1GHz |
55 [-] Show Supplier Material materials with Verlustfaktor of 55 [-] | dry | IEC 60250 | 5GHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Pipe Fittings, Hydrogen fuel cells | |
Certifications | Food Contact, Drinking Water | |
Fillers | 40% Glass Fiber |