Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.62 g/cm³ Show Supplier Material materials with Dichte of 1.62 g/cm³ | dry | ISO 1183 |
Wasserabsorption | 3.3 % Show Supplier Material materials with Wasserabsorption of 3.3 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 17.5 GPa Show Supplier Material materials with Biegemodul of 17.5 GPa | dry | ISO 178 | |
120 °C | 16.3 GPa Show Supplier Material materials with Biegemodul of 16.3 GPa | dry | ISO 178 | |
160 °C | 8.5 GPa Show Supplier Material materials with Biegemodul of 8.5 GPa | dry | ISO 178 | |
180 °C | 6.7 GPa Show Supplier Material materials with Biegemodul of 6.7 GPa | dry | ISO 178 | |
200 °C | 6.2 GPa Show Supplier Material materials with Biegemodul of 6.2 GPa | dry | ISO 178 | |
210 °C | 6 GPa Show Supplier Material materials with Biegemodul of 6 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 2.3 % Show Supplier Material materials with Dehnung of 2.3 % | dry | ISO 527-1/-2 |
2.1 % Show Supplier Material materials with Dehnung of 2.1 % | dry | ISO 527-1/-2 | ||
40 °C | 2.1 % Show Supplier Material materials with Dehnung of 2.1 % | dry | ISO 527-1/-2 | |
80 °C | 2.2 % Show Supplier Material materials with Dehnung of 2.2 % | dry | ISO 527-1/-2 | |
100 °C | 2.3 % Show Supplier Material materials with Dehnung of 2.3 % | dry | ISO 527-1/-2 | |
120 °C | 2.4 % Show Supplier Material materials with Dehnung of 2.4 % | dry | ISO 527-1/-2 | |
150 °C | 5 % Show Supplier Material materials with Dehnung of 5 % | dry | ISO 527-1/-2 | |
160 °C | 6 % Show Supplier Material materials with Dehnung of 6 % | dry | ISO 527-1/-2 | |
180 °C | 6 % Show Supplier Material materials with Dehnung of 6 % | dry | ISO 527-1/-2 | |
200 °C | 6 % Show Supplier Material materials with Dehnung of 6 % | dry | ISO 527-1/-2 | |
210 °C | 0.006 % Show Supplier Material materials with Dehnung of 0.006 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 19 GPa Show Supplier Material materials with Elastizitätsmodul of 19 GPa | dry | ISO 527-1/-2 |
18 GPa Show Supplier Material materials with Elastizitätsmodul of 18 GPa | dry | ISO 527-1/-2 | ||
40 °C | 17.5 GPa Show Supplier Material materials with Elastizitätsmodul of 17.5 GPa | dry | ISO 527-1/-2 | |
80 °C | 17 GPa Show Supplier Material materials with Elastizitätsmodul of 17 GPa | dry | ISO 527-1/-2 | |
100 °C | 16.8 GPa Show Supplier Material materials with Elastizitätsmodul of 16.8 GPa | dry | ISO 527-1/-2 | |
120 °C | 16 GPa Show Supplier Material materials with Elastizitätsmodul of 16 GPa | dry | ISO 527-1/-2 | |
150 °C | 9 GPa Show Supplier Material materials with Elastizitätsmodul of 9 GPa | dry | ISO 527-1/-2 | |
160 °C | 7.7 GPa Show Supplier Material materials with Elastizitätsmodul of 7.7 GPa | dry | ISO 527-1/-2 | |
180 °C | 6.2 GPa Show Supplier Material materials with Elastizitätsmodul of 6.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 5.8 GPa Show Supplier Material materials with Elastizitätsmodul of 5.8 GPa | dry | ISO 527-1/-2 | |
210 °C | 5.6 GPa Show Supplier Material materials with Elastizitätsmodul of 5.6 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 390 MPa Show Supplier Material materials with Flexural yield strength of 390 MPa | dry | ISO 178 | |
120 °C | 270 MPa Show Supplier Material materials with Flexural yield strength of 270 MPa | dry | ISO 178 | |
160 °C | 145 MPa Show Supplier Material materials with Flexural yield strength of 145 MPa | dry | ISO 178 | |
180 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
200 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |
210 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry | ISO 179/1eA |
23 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | dry | ISO 179/1eU |
23 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 320 MPa Show Supplier Material materials with Zugfestigkeit of 320 MPa | dry | ISO 527-1/-2 |
260 MPa Show Supplier Material materials with Zugfestigkeit of 260 MPa | dry | ISO 527-1/-2 | ||
40 °C | 245 MPa Show Supplier Material materials with Zugfestigkeit of 245 MPa | dry | ISO 527-1/-2 | |
80 °C | 205 MPa Show Supplier Material materials with Zugfestigkeit of 205 MPa | dry | ISO 527-1/-2 | |
100 °C | 195 MPa Show Supplier Material materials with Zugfestigkeit of 195 MPa | dry | ISO 527-1/-2 | |
120 °C | 170 MPa Show Supplier Material materials with Zugfestigkeit of 170 MPa | dry | ISO 527-1/-2 | |
150 °C | 100 MPa Show Supplier Material materials with Zugfestigkeit of 100 MPa | dry | ISO 527-1/-2 | |
160 °C | 96 MPa Show Supplier Material materials with Zugfestigkeit of 96 MPa | dry | ISO 527-1/-2 | |
180 °C | 75 MPa Show Supplier Material materials with Zugfestigkeit of 75 MPa | dry | ISO 527-1/-2 | |
200 °C | 65 MPa Show Supplier Material materials with Zugfestigkeit of 65 MPa | dry | ISO 527-1/-2 | |
210 °C | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Glasübergangstemperatur | 155 °C Show Supplier Material materials with Glasübergangstemperatur of 155 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | ||
Glow Wire Flammability Index | 700 °C Show Supplier Material materials with Glow Wire Flammability Index of 700 °C | dry | IEC 60695-2-12 | 2 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | |||
Glow Wire Ignition Temperature | 725 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 725 °C | dry | IEC 60695-2-13 | 2 mm | ||
825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | IEC 60695-2-13 | 3 mm | |||
Koeffizient der thermischen Ausdehnung | 1.4e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
4.7e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4.7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Schmelzpunkt | 330 °C Show Supplier Material materials with Schmelzpunkt of 330 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 305 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 305 °C | dry | ISO 75-1/-2 | 2 MPa | ||
320 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 320 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Structural Parts with ForTii® Ace, Timing drive systems | |
Fillers | 50% Glass Fiber |