Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.13 g/cm³ Show Supplier Material materials with Dichte of 1.13 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.8 % Show Supplier Material materials with Moisture absorption of 2.8 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 0.99 GPa Show Supplier Material materials with Biegemodul of 0.99 GPa | conditioned | ISO 178 | |
3 GPa Show Supplier Material materials with Biegemodul of 3 GPa | dry | ISO 178 | ||
Elastizitätsmodul | 1 GPa Show Supplier Material materials with Elastizitätsmodul of 1 GPa | conditioned | ISO 527-1/-2 | |
3.1 GPa Show Supplier Material materials with Elastizitätsmodul of 3.1 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 5.3 % Show Supplier Material materials with Elongation at yield of 5.3 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 40 MPa Show Supplier Material materials with Flexural yield strength of 40 MPa | conditioned | ISO 178 | |
119 MPa Show Supplier Material materials with Flexural yield strength of 119 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | 23 °C | 4 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4 kJ/m² | dry | ISO 179/1eA |
23 °C | 31 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 31 kJ/m² | conditioned | ISO 179/1eA |
Thermisch
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Entflammbarkeit | V-2 | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Koeffizient der thermischen Ausdehnung | 6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | 0.81 mm | UL746B | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | 0.81 mm | UL746B | ||
Relative temperature index, mechanical strength | 80 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C | dry | 0.81 mm | UL746B | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Wärmeformbeständigkeitstemperatur | 57 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 57 °C | dry | ISO 75-1/-2 | 2 MPa | ||
175 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 175 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
Durchschlagfestigkeit | 26 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 26 kV/mm | dry | IEC 60243-1 | |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Surface resistivity | 2e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 2e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 220 [-] Show Supplier Material materials with Verlustfaktor of 220 [-] | dry | IEC 62631-2-1 | 1MHz |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Schmelzmassenflussrate | 230 °C | 34 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 34 g/10min | dry | ISO 1133 | |
Schmelzvolumenflussrate | 230 °C | 30 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 30 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 1.2 % Show Supplier Material materials with Schrumpfung of 1.2 % | dry | ISO 294-4 | Parallel | |
1.3 % Show Supplier Material materials with Schrumpfung of 1.3 % | dry | ISO 294-4 | Normal | ||
Viscosity number | 138 cm³/gr Show Supplier Material materials with Viscosity number of 138 cm³/gr | dry | ISO 307, 1157, 1628 |