Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.18 g/cm³ Show Supplier Material materials with Dichte of 1.18 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.5 % Show Supplier Material materials with Moisture absorption of 2.5 % | dry | Sim. to ISO 62 |
Sauerstoffindex | 40 % Show Supplier Material materials with Sauerstoffindex of 40 % | dry | ISO 4589-1/-2 |
Wasserabsorption | 9 % Show Supplier Material materials with Wasserabsorption of 9 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 1.3 GPa Show Supplier Material materials with Biegemodul of 1.3 GPa | conditioned | ISO 178 | |
3.4 GPa Show Supplier Material materials with Biegemodul of 3.4 GPa | dry | ISO 178 | ||
Dehnung | 6 % Show Supplier Material materials with Dehnung of 6 % | dry | ISO 527-1/-2 | |
50 % Show Supplier Material materials with Dehnung of 50 % | conditioned | ISO 527-1/-2 | ||
90 °C | 50 % Show Supplier Material materials with Dehnung of 50 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 1.4 GPa Show Supplier Material materials with Elastizitätsmodul of 1.4 GPa | conditioned | ISO 527-1/-2 | |
3.8 GPa Show Supplier Material materials with Elastizitätsmodul of 3.8 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 3.5 % Show Supplier Material materials with Elongation at yield of 3.5 % | dry | ISO 527-1/-2 | |
22 % Show Supplier Material materials with Elongation at yield of 22 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 40 MPa Show Supplier Material materials with Flexural yield strength of 40 MPa | conditioned | ISO 178 | |
115 MPa Show Supplier Material materials with Flexural yield strength of 115 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 95 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 95 kJ/m² | dry | ISO 179/1eU |
Thermisch
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Ball pressure temperature | 210 °C Show Supplier Material materials with Ball pressure temperature of 210 °C | dry | IEC 60695-10-2 | |||
Entflammbarkeit | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Koeffizient der thermischen Ausdehnung | 9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
9e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Relative temperature index, electrical | 150 °C Show Supplier Material materials with Relative temperature index, electrical of 150 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 75 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 75 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 95 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 95 °C | dry | UL746B | 0.75 mm | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperaturleitfähigkeit | 1.22e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.22e-07 mm²/s | dry | - | |||
Vicat-Erweichungstemperatur | 204 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 204 °C | dry | ISO 306 | 50°C/h 50N | ||
Wärmeformbeständigkeitstemperatur | 75 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 75 °C | dry | ISO 75-1/-2 | 2 MPa | ||
180 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 180 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.2 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.2 [-] | dry | IEC 62631-2-1 | 1MHz |
3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
3.6 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.6 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 8 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry, conditioned | IEC 60112 | |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 90 [-] Show Supplier Material materials with Verlustfaktor of 90 [-] | dry | IEC 62631-2-1 | 100Hz |
200 [-] Show Supplier Material materials with Verlustfaktor of 200 [-] | dry | IEC 62631-2-1 | 1MHz | |
800 [-] Show Supplier Material materials with Verlustfaktor of 800 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
1250 [-] Show Supplier Material materials with Verlustfaktor of 1250 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 898 g/cm³ Show Supplier Material materials with Density of melt of 898 g/cm³ | dry | - | ||
Schmelzvolumenflussrate | 250 °C | 34.8 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 34.8 cm³/10min | dry | ISO 1133 | |
Schrumpfung | 0.91 % Show Supplier Material materials with Schrumpfung of 0.91 % | dry | ISO 294-4 | Normal | |
1.1 % Show Supplier Material materials with Schrumpfung of 1.1 % | dry | ISO 294-4 | Parallel | ||
Specific heat capacity melt | 2530 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2530 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.28 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.28 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Contactors, Motor Starter/Overload Relays, Fuse holder | |
Certifications | VDE, Yellow Card Available |