Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.29 g/cm³ Show Supplier Material materials with Dichte of 1.29 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Wasserabsorption | 0.6 % Show Supplier Material materials with Wasserabsorption of 0.6 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Biegemodul | 0.94 GPa Show Supplier Material materials with Biegemodul of 0.94 GPa | dry | ISO 178 | |
Dehnung | 300 % Show Supplier Material materials with Dehnung of 300 % | dry | ISO 527-1/-2 | |
360 % Show Supplier Material materials with Dehnung of 360 % | dry | ISO 527-1/-2 | ||
570 % Show Supplier Material materials with Dehnung of 570 % | dry | ISO 527-1/-2 | ||
Elastizitätsmodul | 0.9 GPa Show Supplier Material materials with Elastizitätsmodul of 0.9 GPa | dry | ISO 527-1/-2 | |
Härte, Shore D | 71 [-] Show Supplier Material materials with Härte, Shore D of 71 [-] | dry | ISO 868 | 3s |
Reißfestigkeit | 224 kN/m Show Supplier Material materials with Reißfestigkeit of 224 kN/m | dry | ISO 34-1; Method B | |
228 kN/m Show Supplier Material materials with Reißfestigkeit of 228 kN/m | dry | ISO 34-1; Method B | ||
Zugfestigkeit | 45 MPa Show Supplier Material materials with Zugfestigkeit of 45 MPa | dry | ISO 527-1/-2 | |
58.0 MPa Show Supplier Material materials with Zugfestigkeit of 58.0 MPa | dry | ISO 527-1/-2 | Normal |
Thermisch
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.8 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.8 [-] | dry | IEC 62631-2-1 | 1MHz |
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | dry | IEC 60112 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Schmelzvolumenflussrate | 230 °C | 4 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 4 cm³/10min | dry | ISO 1133 |
Technological properties
Property |
---|