Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.32 g/cm³ Show Supplier Material materials with Dichte of 1.32 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 2.4 % Show Supplier Material materials with Wasserabsorption of 2.4 % | dry | ISO 62 | at 23°C after 24h |
8.7 % Show Supplier Material materials with Wasserabsorption of 8.7 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 22 GPa Show Supplier Material materials with Biegemodul of 22 GPa | dry | ISO 178 | |
Dehnung | 1.6 % Show Supplier Material materials with Dehnung of 1.6 % | dry | ISO 527-1/-2 | |
3.5 % Show Supplier Material materials with Dehnung of 3.5 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3.1 % Show Supplier Material materials with Dehnung of 3.1 % | dry | ISO 527-1/-2 | |
160 °C | 3.1 % Show Supplier Material materials with Dehnung of 3.1 % | dry | ISO 527-1/-2 | |
180 °C | 3.1 % Show Supplier Material materials with Dehnung of 3.1 % | dry | ISO 527-1/-2 | |
200 °C | 3.1 % Show Supplier Material materials with Dehnung of 3.1 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 14.5 GPa Show Supplier Material materials with Elastizitätsmodul of 14.5 GPa | conditioned | ISO 527-1/-2 | |
24 GPa Show Supplier Material materials with Elastizitätsmodul of 24 GPa | dry | ISO 527-1/-2 | ||
120 °C | 13.5 GPa Show Supplier Material materials with Elastizitätsmodul of 13.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 12 GPa Show Supplier Material materials with Elastizitätsmodul of 12 GPa | dry | ISO 527-1/-2 | |
180 °C | 11.5 GPa Show Supplier Material materials with Elastizitätsmodul of 11.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 365 MPa Show Supplier Material materials with Flexural yield strength of 365 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 7 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | dry | ISO 179/1eA | |
23 °C | 17 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 17 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | dry | ISO 179/1eU |
-30 °C | 55.0 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 55.0 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 50 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 50 kJ/m² | dry | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 80 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 170 MPa Show Supplier Material materials with Zugfestigkeit of 170 MPa | conditioned | ISO 527-1/-2 | |
260 MPa Show Supplier Material materials with Zugfestigkeit of 260 MPa | dry | ISO 527-1/-2 | ||
120 °C | 140 MPa Show Supplier Material materials with Zugfestigkeit of 140 MPa | dry | ISO 527-1/-2 | |
160 °C | 115 MPa Show Supplier Material materials with Zugfestigkeit of 115 MPa | dry | ISO 527-1/-2 | |
180 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | dry | ISO 527-1/-2 | |
200 °C | 95 MPa Show Supplier Material materials with Zugfestigkeit of 95 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 2.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
3.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 290 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 290 °C | dry | ISO 75-1/-2 | 2 MPa |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schrumpfung | 0.3 % Show Supplier Material materials with Schrumpfung of 0.3 % | dry | ISO 294-4 | Parallel |
0.7 % Show Supplier Material materials with Schrumpfung of 0.7 % | dry | ISO 294-4 | Normal | |
Viscosity number | 150 cm³/gr Show Supplier Material materials with Viscosity number of 150 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | CRB Cap, CRB Housing, Gears, Electronic throttle control actuators, Exhaust gas recirculation actuators, Turbo actuators, Coolant valve actuators | |
Fillers | 30% Carbon Fiber and PTFE |