Allgemein
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dichte | 1.53 g/cm³ Show Supplier Material materials with Dichte of 1.53 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.2 % Show Supplier Material materials with Moisture absorption of 2.2 % | dry | Sim. to ISO 62 | |
Wasserabsorption | 2.1 % Show Supplier Material materials with Wasserabsorption of 2.1 % | dry | ISO 62 | at 23°C after 24h |
7.4 % Show Supplier Material materials with Wasserabsorption of 7.4 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 6 GPa Show Supplier Material materials with Biegemodul of 6 GPa | conditioned | ISO 178 | |
9 GPa Show Supplier Material materials with Biegemodul of 9 GPa | dry | ISO 178 | ||
120 °C | 5.4 GPa Show Supplier Material materials with Biegemodul of 5.4 GPa | dry | ISO 178 | |
160 °C | 5 GPa Show Supplier Material materials with Biegemodul of 5 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3.2 % Show Supplier Material materials with Dehnung of 3.2 % | conditioned | ISO 527-1/-2 |
-40 °C | 3.3 % Show Supplier Material materials with Dehnung of 3.3 % | dry | ISO 527-1/-2 | |
3.4 % Show Supplier Material materials with Dehnung of 3.4 % | dry | ISO 527-1/-2 | ||
6 % Show Supplier Material materials with Dehnung of 6 % | conditioned | ISO 527-1/-2 | ||
120 °C | 6.5 % Show Supplier Material materials with Dehnung of 6.5 % | dry | ISO 527-1/-2 | |
160 °C | 6.5 % Show Supplier Material materials with Dehnung of 6.5 % | dry | ISO 527-1/-2 | |
180 °C | 6.5 % Show Supplier Material materials with Dehnung of 6.5 % | dry | ISO 527-1/-2 | |
200 °C | 6.5 % Show Supplier Material materials with Dehnung of 6.5 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry | ISO 527-1/-2 |
-40 °C | 12 GPa Show Supplier Material materials with Elastizitätsmodul of 12 GPa | conditioned | ISO 527-1/-2 | |
6.6 GPa Show Supplier Material materials with Elastizitätsmodul of 6.6 GPa | conditioned | ISO 527-1/-2 | ||
10.5 GPa Show Supplier Material materials with Elastizitätsmodul of 10.5 GPa | dry | ISO 527-1/-2 | ||
120 °C | 5.2 GPa Show Supplier Material materials with Elastizitätsmodul of 5.2 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.8 GPa Show Supplier Material materials with Elastizitätsmodul of 4.8 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.5 GPa Show Supplier Material materials with Elastizitätsmodul of 4.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.2 GPa Show Supplier Material materials with Elastizitätsmodul of 4.2 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | conditioned | ISO 178 | |
280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | ||
120 °C | 135 MPa Show Supplier Material materials with Flexural yield strength of 135 MPa | dry | ISO 178 | |
160 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 11 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 11 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 13 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 13 kJ/m² | dry | ISO 179/1eA | |
23 °C | 17 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 17 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 65 kJ/m² | dry | ISO 179/1eU |
-30 °C | 70 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 70 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | dry | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 235 MPa Show Supplier Material materials with Zugfestigkeit of 235 MPa | conditioned | ISO 527-1/-2 |
-40 °C | 250 MPa Show Supplier Material materials with Zugfestigkeit of 250 MPa | dry | ISO 527-1/-2 | |
130 MPa Show Supplier Material materials with Zugfestigkeit of 130 MPa | conditioned | ISO 527-1/-2 | ||
200 MPa Show Supplier Material materials with Zugfestigkeit of 200 MPa | dry | ISO 527-1/-2 | ||
120 °C | 100 MPa Show Supplier Material materials with Zugfestigkeit of 100 MPa | dry | ISO 527-1/-2 | |
160 °C | 85 MPa Show Supplier Material materials with Zugfestigkeit of 85 MPa | dry | ISO 527-1/-2 | |
180 °C | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | dry | ISO 527-1/-2 | |
200 °C | 75 MPa Show Supplier Material materials with Zugfestigkeit of 75 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glasübergangstemperatur | 75 °C Show Supplier Material materials with Glasübergangstemperatur of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Koeffizient der thermischen Ausdehnung | 2.5e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 295 °C Show Supplier Material materials with Schmelzpunkt of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperaturleitfähigkeit | 1.26e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.26e-07 mm²/s | dry | - | ||
Vicat-Erweichungstemperatur | 290 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 290 °C | dry | ISO 306 | 50°C/h 50N | |
Wärmeformbeständigkeitstemperatur | 290 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 290 °C | dry | ISO 75-1/-2 | 2 MPa | |
290 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard |
---|---|---|---|
Kriechstromfestigkeit | 400 V Show Supplier Material materials with Kriechstromfestigkeit of 400 V | dry | IEC 60112 |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+07 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+07 Ω·cm | conditioned | IEC 62631-3-1 |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1320 g/cm³ Show Supplier Material materials with Density of melt of 1320 g/cm³ | dry | - | |
Schrumpfung | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | dry | Sim. to ISO 294-4 | Parallel |
1.3 % Show Supplier Material materials with Schrumpfung of 1.3 % | dry | Sim. to ISO 294-4 | Normal | |
Specific heat capacity melt | 1890 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1890 J/(kg·K) | dry | - | |
Spiral flow length | 105 | dry | - | 1.0 mm 800 bar |
115 | dry | - | 1.0 mm 900 bar | |
125 | dry | - | 1.0 mm 1000 bar | |
Thermal conductivity of melt | 0.319 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.319 W/(m·K) | dry | - | |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Self propelled lawnmower transmission gears, Transmission Control Gears, Oil Pump Gears (2-wheelers), Rod Guides, MTF/DMF Components, Crankshaft Balance Gears, Oil Pump Gears (automotive), EPS gears, Power Lift Gate Actuators, Power Door Actuators, Power Window Actuators, Windshield Wiper Actuators, EPS Steering components: Gears, Flex couplers and Sensors, CRB Housing, Gears, Electronic throttle control actuators, Exhaust gas recirculation actuators, Turbo actuators, Coolant valve actuators | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber and PTFE |