Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.1 g/cm³ Show Supplier Material materials with Dichte of 1.1 g/cm³ | dry | ISO 1183 |
Moisture absorption | 3 % Show Supplier Material materials with Moisture absorption of 3 % | dry | Sim. to ISO 62 |
Wasserabsorption | 9 % Show Supplier Material materials with Wasserabsorption of 9 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | 2.5 GPa Show Supplier Material materials with Elastizitätsmodul of 2.5 GPa | dry | ISO 527-1/-2 | |
Elongation at yield | 4 % Show Supplier Material materials with Elongation at yield of 4 % | dry | ISO 527-1/-2 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 20 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 20 kJ/m² | dry | ISO 179/1eA |
23 °C | 50 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 50 kJ/m² | dry | ISO 179/1eA |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.4e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperaturleitfähigkeit | 9.28e-08 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 9.28e-08 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 60 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 60 °C | dry | ISO 75-1/-2 | 2 MPa | |
170 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 170 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Density of melt | 915 g/cm³ Show Supplier Material materials with Density of melt of 915 g/cm³ | dry | - | |
Schmelzvolumenflussrate | 275 °C | 33 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 33 cm³/10min | dry | ISO 1133 |
Specific heat capacity melt | 2710 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2710 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.23 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.23 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Clean Air Inlet Ducts, Hot Charged Air Ducts, Cold Charged Air Ducts |