Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.2 g/cm³ Show Supplier Material materials with Dichte of 1.2 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2 % Show Supplier Material materials with Moisture absorption of 2 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6.8 % Show Supplier Material materials with Wasserabsorption of 6.8 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 4 % Show Supplier Material materials with Dehnung of 4 % | dry | ISO 527-1/-2 | |
15 % Show Supplier Material materials with Dehnung of 15 % | conditioned | ISO 527-1/-2 | ||
Elastizitätsmodul | 2.6 GPa Show Supplier Material materials with Elastizitätsmodul of 2.6 GPa | conditioned | ISO 527-1/-2 | |
5.4 GPa Show Supplier Material materials with Elastizitätsmodul of 5.4 GPa | dry | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 9 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 9 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | dry | ISO 179/1eA | |
23 °C | 25 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 25 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 70 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 70 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 70 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 70 kJ/m² | dry | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | 60 MPa Show Supplier Material materials with Zugfestigkeit of 60 MPa | conditioned | ISO 527-1/-2 | |
105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 3e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
8e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Wärmeformbeständigkeitstemperatur | 185 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 185 °C | dry | ISO 75-1/-2 | 2 MPa | |
205 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 205 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.6 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.6 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 20 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 20 kV/mm | conditioned | IEC 60243-1 | |
25 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 25 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 100 [-] Show Supplier Material materials with Verlustfaktor of 100 [-] | dry | IEC 62631-2-1 | 100Hz |
180 [-] Show Supplier Material materials with Verlustfaktor of 180 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
1500 [-] Show Supplier Material materials with Verlustfaktor of 1500 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Technological properties
Property | ||
---|---|---|
Fillers | 15% Glass Fiber |