Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.35 g/cm³ Show Supplier Material materials with Dichte of 1.35 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 |
Wasserabsorption | 6 % Show Supplier Material materials with Wasserabsorption of 6 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 5.5 GPa Show Supplier Material materials with Biegemodul of 5.5 GPa | conditioned | ISO 178 | |
9 GPa Show Supplier Material materials with Biegemodul of 9 GPa | dry | ISO 178 | ||
120 °C | 4 GPa Show Supplier Material materials with Biegemodul of 4 GPa | dry | ISO 178 | |
160 °C | 3.7 GPa Show Supplier Material materials with Biegemodul of 3.7 GPa | dry | ISO 178 | |
Dehnung | -40 °C | 3.1 % Show Supplier Material materials with Dehnung of 3.1 % | dry | ISO 527-1/-2 |
3.3 % Show Supplier Material materials with Dehnung of 3.3 % | dry | ISO 527-1/-2 | ||
7 % Show Supplier Material materials with Dehnung of 7 % | conditioned | ISO 527-1/-2 | ||
120 °C | 9.3 % Show Supplier Material materials with Dehnung of 9.3 % | dry | ISO 527-1/-2 | |
150 °C | 8.9 % Show Supplier Material materials with Dehnung of 8.9 % | dry | ISO 527-1/-2 | |
160 °C | 8.8 % Show Supplier Material materials with Dehnung of 8.8 % | dry | ISO 527-1/-2 | |
180 °C | 8.6 % Show Supplier Material materials with Dehnung of 8.6 % | dry | ISO 527-1/-2 | |
200 °C | 8.4 % Show Supplier Material materials with Dehnung of 8.4 % | dry | ISO 527-1/-2 | |
Elastizitätsmodul | -40 °C | 10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | dry | ISO 527-1/-2 |
5.7 GPa Show Supplier Material materials with Elastizitätsmodul of 5.7 GPa | conditioned | ISO 527-1/-2 | ||
9.5 GPa Show Supplier Material materials with Elastizitätsmodul of 9.5 GPa | dry | ISO 527-1/-2 | ||
100 °C | 4.2 GPa Show Supplier Material materials with Elastizitätsmodul of 4.2 GPa | dry | ISO 527-1/-2 | |
120 °C | 3.9 GPa Show Supplier Material materials with Elastizitätsmodul of 3.9 GPa | dry | ISO 527-1/-2 | |
150 °C | 3.5 GPa Show Supplier Material materials with Elastizitätsmodul of 3.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.3 GPa Show Supplier Material materials with Elastizitätsmodul of 3.3 GPa | dry | ISO 527-1/-2 | |
180 °C | 3.0 GPa Show Supplier Material materials with Elastizitätsmodul of 3.0 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.6 GPa Show Supplier Material materials with Elastizitätsmodul of 2.6 GPa | dry | ISO 527-1/-2 | |
Flexural yield strength | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | conditioned | ISO 178 | |
270 MPa Show Supplier Material materials with Flexural yield strength of 270 MPa | dry | ISO 178 | ||
120 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |
160 °C | 88 MPa Show Supplier Material materials with Flexural yield strength of 88 MPa | dry | ISO 178 | |
Schlagfestigkeit, Charpy gekerbt | -30 °C | 10 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 12.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 12.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 22 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 22 kJ/m² | conditioned | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 65 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | dry | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 90 kJ/m² | conditioned | ISO 179/1eU | |
Zugfestigkeit | -40 °C | 220 MPa Show Supplier Material materials with Zugfestigkeit of 220 MPa | dry | ISO 527-1/-2 |
105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | conditioned | ISO 527-1/-2 | ||
175 MPa Show Supplier Material materials with Zugfestigkeit of 175 MPa | dry | ISO 527-1/-2 | ||
100 °C | 87 MPa Show Supplier Material materials with Zugfestigkeit of 87 MPa | dry | ISO 527-1/-2 | |
120 °C | 82 MPa Show Supplier Material materials with Zugfestigkeit of 82 MPa | dry | ISO 527-1/-2 | |
150 °C | 70 MPa Show Supplier Material materials with Zugfestigkeit of 70 MPa | dry | ISO 527-1/-2 | |
160 °C | 65 MPa Show Supplier Material materials with Zugfestigkeit of 65 MPa | dry | ISO 527-1/-2 | |
180 °C | 50 MPa Show Supplier Material materials with Zugfestigkeit of 50 MPa | dry | ISO 527-1/-2 | |
200 °C | 40 MPa Show Supplier Material materials with Zugfestigkeit of 40 MPa | dry | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
7e-07 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperaturleitfähigkeit | 1.08e-07 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 1.08e-07 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 200 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 200 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.3 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Kriechstromfestigkeit | 500 V Show Supplier Material materials with Kriechstromfestigkeit of 500 V | conditioned | IEC 60112 | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 50 [-] Show Supplier Material materials with Verlustfaktor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Verlustfaktor of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Verlustfaktor of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 1120 g/cm³ Show Supplier Material materials with Density of melt of 1120 g/cm³ | dry | - | ||
Schmelzmassenflussrate | 275 °C | 55.0 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 55.0 g/10min | dry | ISO 1133 | |
Schrumpfung | 0.3 % Show Supplier Material materials with Schrumpfung of 0.3 % | dry | ISO 294-4 | Parallel | |
1.1 % Show Supplier Material materials with Schrumpfung of 1.1 % | dry | ISO 294-4 | Normal | ||
Specific heat capacity melt | 2250 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2250 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.27 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.27 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Air inlet manifolds, Temperature Sensor, Speed Sensor, Positition Sensor | |
Fillers | 30% Glass Fiber |