Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.12 g/cm³ Show Supplier Material materials with Dichte of 1.12 g/cm³ | dry | ISO 1183 |
Moisture absorption | 3.8 % Show Supplier Material materials with Moisture absorption of 3.8 % | dry | Sim. to ISO 62 |
Wasserabsorption | 13 % Show Supplier Material materials with Wasserabsorption of 13 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Biegemodul | 0.47 GPa Show Supplier Material materials with Biegemodul of 0.47 GPa | conditioned | ISO 178 | |
2.4 GPa Show Supplier Material materials with Biegemodul of 2.4 GPa | dry | ISO 178 | ||
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | dry, conditioned | ISO 527-1/-2 | |
Elastizitätsmodul | 0.44 GPa Show Supplier Material materials with Elastizitätsmodul of 0.44 GPa | conditioned | ISO 527-1/-2 | |
2.3 GPa Show Supplier Material materials with Elastizitätsmodul of 2.3 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 4.5 % Show Supplier Material materials with Elongation at yield of 4.5 % | dry | ISO 527-1/-2 | |
24 % Show Supplier Material materials with Elongation at yield of 24 % | conditioned | ISO 527-1/-2 | ||
Flexural yield strength | 23 MPa Show Supplier Material materials with Flexural yield strength of 23 MPa | conditioned | ISO 178 | |
95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 3.2 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 3.2 kJ/m² | dry | ISO 179/1eA | |
23 °C | 4.3 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 4.3 kJ/m² | dry | ISO 179/1eA | |
Zugfestigkeit | 42 MPa Show Supplier Material materials with Zugfestigkeit of 42 MPa | dry | ISO 527-1/-2 | |
46 MPa Show Supplier Material materials with Zugfestigkeit of 46 MPa | conditioned | ISO 527-1/-2 |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Schmelzpunkt | 200 °C Show Supplier Material materials with Schmelzpunkt of 200 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Wärmeformbeständigkeitstemperatur | 51 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 51 °C | dry | ISO 75-1/-2 | 2 MPa | |
84 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 84 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Schmelzmassenflussrate | 230 °C | 2.6 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 2.6 g/10min | dry | ISO 1133 |
Schmelzvolumenflussrate | 230 °C | 2.3 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 2.3 cm³/10min | dry | ISO 1133 |
Technological properties
Property |
---|