Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.11 g/cm³ Show Supplier Material materials with Dichte of 1.11 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.5 % Show Supplier Material materials with Moisture absorption of 2.5 % | dry | Sim. to ISO 62 |
Wasserabsorption | 9 % Show Supplier Material materials with Wasserabsorption of 9 % | dry | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | dry, conditioned | ISO 527-1/-2 | |
Elastizitätsmodul | 0.75 GPa Show Supplier Material materials with Elastizitätsmodul of 0.75 GPa | conditioned | ISO 527-1/-2 | |
2.5 GPa Show Supplier Material materials with Elastizitätsmodul of 2.5 GPa | dry | ISO 527-1/-2 | ||
Elongation at yield | 4 % Show Supplier Material materials with Elongation at yield of 4 % | dry | ISO 527-1/-2 | |
25 % Show Supplier Material materials with Elongation at yield of 25 % | conditioned | ISO 527-1/-2 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 16 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 16 kJ/m² | dry | ISO 179/1eA | |
23 °C | 28.0 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 28.0 kJ/m² | conditioned | ISO 179/1eA |
Thermisch
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.4e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Temperaturleitfähigkeit | 9.28e-08 mm²/s Show Supplier Material materials with Temperaturleitfähigkeit of 9.28e-08 mm²/s | dry | - | ||
Wärmeformbeständigkeitstemperatur | 55 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 55 °C | dry | ISO 75-1/-2 | 2 MPa | |
130 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 130 °C | dry | ISO 75-1/-2 | 0.45 MPa |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielektrizitätskonstante | 3.1 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.1 [-] | dry | IEC 62631-2-1 | 1MHz |
3.4 [-] Show Supplier Material materials with Dielektrizitätskonstante of 3.4 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielektrizitätskonstante of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Durchschlagfestigkeit | 20 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 20 kV/mm | conditioned | IEC 60243-1 | |
28.0 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 28.0 kV/mm | dry | IEC 60243-1 | ||
Kriechstromfestigkeit | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | conditioned | IEC 60112 | |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Verlustfaktor | 80 [-] Show Supplier Material materials with Verlustfaktor of 80 [-] | dry | IEC 62631-2-1 | 100Hz |
200 [-] Show Supplier Material materials with Verlustfaktor of 200 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Verlustfaktor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Verlustfaktor of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 915 g/cm³ Show Supplier Material materials with Density of melt of 915 g/cm³ | dry | - | |
Schmelzmassenflussrate | 35 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 35 g/10min | dry | ISO 1133 | |
Schrumpfung | 1.37 % Show Supplier Material materials with Schrumpfung of 1.37 % | dry | ISO 294-4 | Parallel |
1.45 % Show Supplier Material materials with Schrumpfung of 1.45 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2710 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2710 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.23 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.23 W/(m·K) | dry | - |
Technological properties
Property |
---|